Technical Data Sheet
physical property | Test Condition | Test Method | Test Result |
---|
melt mass-flow rate | | ASTMD3307 | 42 g/10min |
melt mass-flow rate | | ISO12086 | 42 g/10min |
Water absorption rate | | ASTMD570 | <0.030 % |
hardness | Test Condition | Test Method | Test Result |
---|
| | ASTMD2240 | 55 |
| | ISO868 | 55 |
flammability | Test Condition | Test Method | Test Result |
---|
UL flame retardant rating 3 | | UL94 | V-0 |
Limiting Oxygen Index | | ASTMD2863 | >95 % |
Limiting Oxygen Index | | ISO4589-2 | >95 % |
Supplementary Information | Test Condition | Test Method | Test Result |
---|
CriticalShearRate | | | 12.0 sec^-1 |
MITFoldingEndurance4 | | ASTMD2176 | 4E+03 cycles |
Mechanical properties | Test Condition | Test Method | Test Result |
---|
tensile strength | | ASTMD3307 | 25.0 Mpa |
Tensile stress | | ISO12086 | 25.0 Mpa |
elongation | | ASTMD3307 | 350 % |
Tensile strain | | ISO12086 | 350 % |
Flexural modulus | | ASTMD790 | 690 Mpa |
Flexural modulus | | ISO178 | 690 Mpa |
Electrical performance | Test Condition | Test Method | Test Result |
---|
Volume resistivity | | ASTMD257 | 1E+18 ohms·cm |
Volume resistivity | | ISO1325 | 1E+18 ohms·cm |
Dielectric strength 2 | | ASTMD149 | 80 KV/mm |
Electrical strength | | IEC60243-1 | 80 KV/mm |
dielectric constant | | ASTMD150 | 2.03 |
dielectric constant | | IEC60250 | 2.03 |
Dissipation Factor | | ASTMD150 | <2.0E-4 |
Dissipation Factor | | IEC60250 | <2.0E-4 |
Thermal performance | Test Condition | Test Method | Test Result |
---|
melting temperature | | ASTMD4591 | 305 °C |
IMPORTANT NOTES: Plas.com collected the data in the data sheet from the material manufacturers. Plas.com makes the best effort to improve the accuracy of the data, but has no responsibility for the data. We strongly recommend verifying the validity of the data with the material manufacturers before making a final decision.