TPV Santoprene™ 203-40 CELANESE USA
430
- Unit Price:US$ 4,317 /MT
- Packaging Specification:25 KG/PKG
- Packaging Material:Paper bag
- Supply Quantity:17MT
- Delivery Terms:FOB
- Port of Loading :China Main Port
- Accepted Payment Methods:T/T
- Shipping:Negotiate supplier for shipping details
Supplier Information
ASIA PLASTIC EXCHANGE LIMITED
+86 755 ********View
serv********View
+86 ********View
For more details, please contact the supplier!
Material Description
- Material Properties:dimensional stability |Insulation performance|Recyclable materials|Electrical performance|Superior tear strength|Good colorability|Ozone resistance|Chemical resistance|Fatigue resistance
- Application Areas:Electrical components|diaphragm|Pipe fittings|Movable hinge|Home appliance components|Engine hood parts|Automotive sector|Consumer goods sector|Pipe fittings|diaphragm|Movable hinge|Consumer product application field|Parts under the hood of a car|Application in the automotive field|Electrical components|Home appliance components
- Color:--
- Grade:Injection grade
Technical Data Sheet
| flammability | Test Condition | Test Method | Test Result |
|---|---|---|---|
| UL flame retardant rating | 1.0mm | UL 94 | HB |
| 1.5mm | UL 94 | HB | |
| 3.0mm | UL 94 | HB |
| elastomer | Test Condition | Test Method | Test Result |
|---|---|---|---|
| Permanent compression deformation | 125°C,70hr | ISO 815 | 61 % |
| 70°C,22hr | ISO 815 | 54 % | |
| 125°C,70hr | ASTM D395B | 61 % | |
| 70°C,22hr | ASTM D395B | 54 % | |
| tear strength | 23°C,Across Flow (Across Flow) | ISO 34-1 | 67 kN/m |
| Tensile stress | 100%Strain,23°C,横向Flow | ASTM D412 | 9.00 Mpa |
| 100%Strain,23°C,横向Flow | ISO 37 | 9.00 Mpa | |
| tensile strength | Break,23°C,横向Flow | ASTM D412 | 20.7 Mpa |
| Break,23°C | ISO 37 | 20.7 Mpa | |
| elongation | Break,23°C,Across Flow | ASTM D412 | 610 % |
| Break,23°C,Across Flow | ISO 37 | 610 % | |
| tear strength | 23°C,横向Flow | ASTM D624 | 67.0 kN/m |
| thermal performance | Test Condition | Test Method | Test Result |
|---|---|---|---|
| RTI Str | UL 746 | 85.0 °C | |
| RTI Elec | UL 746 | 85.0 °C | |
| Brittle temperature | ISO 812 | -52.0 °C | |
| ASTM D746 | -52.0 °C |
| Physical properties | Test Condition | Test Method | Test Result |
|---|---|---|---|
| Resistance to cleaning agents | ISO 188 | f4 | |
| UL 749 | f3 |
| Electrical performance | Test Condition | Test Method | Test Result |
|---|---|---|---|
| Dielectric strength | 23°C,2.00mm | ASTM D149 | 28 KV/mm |
| Hot wire ignition | 3.0mm | UL 746 | PLC 2 |
| Dielectric constant | 23°C,1.98mm | ASTM D150 | 2.30 |
| 23°C,1.98mm | IEC 60250 | 2.30 | |
| High voltage arc tracing rate | PLC | UL 746 | |
| Compared to the anti leakage trace index | CTI | UL 746 | PLC 0 |
| Hot wire ignition | 1.0mm | UL 746 | PLC 4 |
| High voltage arc tracing rate | HVTR | UL 746 | PLC 1 |
| Hot wire ignition | 1.5mm | UL 746 | PLC 3 |
| High arc combustion index | HAI | UL 746 | PLC 0 |
| hardness | Test Condition | Test Method | Test Result |
|---|---|---|---|
| Shore hardness | ShoreD,15Sec,23°C | ISO 868 | 41 |
| aging | Test Condition | Test Method | Test Result |
|---|---|---|---|
| Change rate of hardness (Shore) in the air | ShoreA,23°C,168hr,inTrichloroethylene | ASTM D471 | 1.0 |
| ShoreA,23°C,168hr,inSulfuricAcid,98% | ASTM D471 | 2.0 | |
| ShoreA,23°C,168hr,inSodiumHydroxide,50% | ASTM D471 | 1.0 | |
| ShoreA,23°C,168hr,inSodiumChloride,15% | ASTM D471 | 2.0 | |
| ShoreA,23°C,168hr,inMethylethylketone | ASTM D471 | 0.0 | |
| Change rate of tensile strength in air | 125°C,70hr,inIRM903Oil | ASTM D471 | -27 % |
| 100°C,168hr,inIRM903Oil | ASTM D471 | -26 % | |
| 100°C,168hr,inDeionizedWater | ASTM D471 | 3.0 % | |
| 23°C,168hr,inTrichloroethylene | ASTM D471 | 8.0 % | |
| 23°C,168hr,inSulfuricAcid,98% | ASTM D471 | -22 % | |
| 23°C,168hr,inSodiumHydroxide,50% | ASTM D471 | 4.0 % | |
| 23°C,168hr,inSodiumChloride,15% | ASTM D471 | 4.0 % | |
| 23°C,168hr,inMethylethylketone | ASTM D471 | 3.0 % | |
| 23°C,168hr,inIsopropylAlcohol | ASTM D471 | 5.0 % | |
| 23°C,168hr,inHydrochloricAcid,10% | ASTM D471 | 6.0 % | |
| Change rate of hardness (Shore) in the air | ShoreA,100°C,168hr,inDeionizedWater | ASTM D471 | 0.0 |
| ShoreA,100°C,168hr,inIRM903Oil | ASTM D471 | -13 | |
| ShoreA,125°C,168hr,inIRM903Oil | ASTM D471 | -15 | |
| Shore hardness | ShoreA,23°C,168hr,inAceticAcid | ISO 1817 | -1.0 |
| ShoreA,23°C,168hr,inCyclohexane | ISO 1817 | -13 | |
| Quality change rate | 23°C,168hr,inSulfuricAcid,98% | ASTM D471 | 1.1 % |
| 23°C,168hr,inTrichloroethylene | ASTM D471 | -1.0 % | |
| 100°C,168hr,inDeionizedWater | ASTM D471 | 1.4 % | |
| 100°C,168hr,inIRM903Oil | ASTM D471 | 35 % | |
| 125°C,168hr,inIRM903Oil | ASTM D471 | 44 % | |
| 23.0°C,168hr,inMethylethylketone | ISO 1817 | -12 % | |
| Change rate of tensile strength in air | 150°C,168hr | ASTM D573 | -11 % |
| 150°C,168hr | ISO 188 | -11 % | |
| Change rate of ultimate elongation in air | 150°C,168hr | ASTM D573 | -15 % |
| Hardness change rate in the air | ShoreD,150°C,168hr | ASTM D573 | 4.0 |
| Shore hardness | ShoreD,150°C,168hr | ISO 188 | 4.0 |
| Change rate of tensile strength in air | 23°C,168hr,inAceticAcid | ASTM D471 | 0.0 % |
| 23°C,168hr,inCyclohexane | ASTM D471 | -2.0 % | |
| 23°C,168hr,inDetergent(Tide),2.5% | ASTM D471 | 0.0 % | |
| 23°C,168hr,inEthanol,95% | ASTM D471 | -3.0 % | |
| Tensile stress change rate | 100°C,168hr,inDeionizedWater,Break | ISO 1817 | 0.0 % |
| 100°C,168hr,inIRM903Oil,Break | ISO 1817 | -28 % | |
| 125°C,70hr,inIRM903Oil,Break | ISO 1817 | -33 % | |
| 125°C,168hr,inIRM903Oil,Break | ISO 1817 | -39 % | |
| Change rate of hardness (Shore) in the air | ShoreA,23°C,168hr,inCyclohexane | ASTM D471 | -13 |
| ShoreA,23°C,168hr,inDetergent(Tide),2.5% | ASTM D471 | 0.0 | |
| ShoreA,23°C,168hr,inEthanol,95% | ASTM D471 | 0.0 | |
| ShoreA,23°C,168hr,inHydrochloricAcid,10% | ASTM D471 | -1.0 | |
| ShoreA,23°C,168hr,inIsopropylAlcohol | ASTM D471 | 2.0 | |
| ShoreA,23°C,168hr,inAceticAcid | ASTM D471 | -1.0 | |
| Tensile stress change rate | 23°C,168hr,inCyclohexane,Break | ISO 1817 | 2.0 % |
| 23°C,168hr,inDetergent(Tide),2.5%,Break | ISO 1817 | 0.00.0 % | |
| 23°C,168hr,inEthanol,95%,Break | ISO 1817 | -2.0 % | |
| 23°C,168hr,inHydrochloricAcid,10%,Break | ISO 1817 | 5.0 % | |
| 23°C,168hr,inIsopropylAlcohol,Break | ISO 1817 | 5.0 % | |
| 23°C,168hr,inMethylethylketone,Break | ISO 1817 | 2.0 % | |
| 23°C,168hr,inSodiumChloride,15%,Break | ISO 1817 | 2.0 % | |
| 23°C,168hr,inSodiumHydroxide,50%,Break | ISO 1817 | 3.0 % | |
| 23°C,168hr,inSulfuricAcid,98%,Break | ISO 1817 | -23 % | |
| 23°C,168hr,inTrichloroethylene,Break | ISO 1817 | 2.0 % | |
| Change rate of tensile strength in air | 125°C,168hr,inIRM903Oil | ASTM D471 | -30 % |
| 23°C,168hr,inAceticAcid | ISO 1817 | 0.0 % | |
| 23°C,168hr,inCyclohexane | ISO 1817 | -2.0 % | |
| 23°C,168hr,inDetergent(Tide),2.5% | ISO 1817 | 0.0 % | |
| 23°C,168hr,inEthanol,95% | ISO 1817 | -3.0 % | |
| 23°C,168hr,inIsopropylAlcohol | ISO 1817 | 5.0 % | |
| 23°C,168hr,inMethylethylketone | ISO 1817 | 3.0 % | |
| 23°C,168hr,inHydrochloricAcid,10% | ISO 1817 | 6.0 % | |
| 23°C,168hr,inSodiumChloride,15% | ISO 1817 | 4.0 % | |
| 23°C,168hr,inSodiumHydroxide,50% | ISO 1817 | 4.0 % | |
| Change rate of ultimate elongation in air | 23°C,168hr,inIsopropylAlcohol | ASTM D471 | 5.0 % |
| 23°C,168hr,inMethylethylketone | ASTM D471 | 2.0 % | |
| 23°C,168hr,inSodiumChloride,15% | ASTM D471 | 2.0 % | |
| 23°C,168hr,inSodiumHydroxide,50% | ASTM D471 | 3.0 % | |
| 23°C,168hr,inSulfuricAcid,98% | ASTM D471 | -23 % | |
| 23°C,168hr,inTrichloroethylene | ASTM D471 | 2.0 % | |
| 100°C,168hr,inDeionizedWater | ASTM D471 | 0.0 % | |
| 100°C,168hr,inIRM903Oil | ASTM D471 | -28 % | |
| 125°C,70hr,inIRM903Oil | ASTM D471 | -33 % | |
| 125°C,168hr,inIRM903Oil | ASTM D471 | -39 % | |
| Change rate of tensile strength in air | 23°C,168hr,inSulfuricAcid,98% | ISO 1817 | -22 % |
| Change rate of ultimate elongation in air | 23°C,168hr,inCyclohexane | ASTM D471 | 2.0 % |
| Change rate of tensile strength in air | 23°C,168hr,inTrichloroethylene | ISO 1817 | 8.0 % |
| 100°C,168hr,inDeionizedWater | ISO 1817 | 3.0 % | |
| 100°C,168hr,inIRM903Oil | ISO 1817 | -26 % | |
| 125°C,70hr,inIRM903Oil | ISO 1817 | -27 % | |
| 125°C,168hr,inIRM903Oil | ISO 1817 | -30 % | |
| Change rate of ultimate elongation in air | 23°C,168hr,inDetergent(Tide),2.5% | ASTM D471 | 0.00.0 % |
| 23°C,168hr,inEthanol,95% | ASTM D471 | -2.0 % | |
| 23°C,168hr,inHydrochloricAcid,10% | ASTM D471 | 5.0 % | |
| Shore hardness | ShoreA,23°C,168hr,inDetergent(Tide),2.5% | ISO 1817 | 0.0 |
| ShoreA,23°C,168hr,inEthanol,95% | ISO 1817 | 0.0 | |
| ShoreA,23°C,168hr,inMethylethylketone | ISO 1817 | 0.0 | |
| ShoreA,23°C,168hr,inSodiumChloride,15% | ISO 1817 | 2.0 | |
| ShoreA,23°C,168hr,inSulfuricAcid,98% | ISO 1817 | 2.0 | |
| ShoreA,23°C,168hr,inHydrochloricAcid,10% | ISO 1817 | -1.0 | |
| ShoreA,23°C,168hr,inSodiumHydroxide,50% | ISO 1817 | 1.0 | |
| ShoreA,23°C,168hr,inTrichloroethylene | ISO 1817 | 1.0 | |
| ShoreA,100°C,168hr,inDeionizedWater | ISO 1817 | 0.0 | |
| Quality change rate | 23.0°C,168hr,inCyclohexane | ISO 1817 | -3.4 % |
| Shore hardness | ShoreA,23°C,168hr,inIsopropylAlcohol | ISO 1817 | 2.0 |
| Quality change rate | 23.0°C,168hr,inTrichloroethylene | ISO 1817 | -1.0 % |
| 23.0°C,168hr,inIsopropylAlcohol | ISO 1817 | -5.0 % | |
| 23.0°C,168hr,inEthanol,95% | ISO 1817 | -0.60 % | |
| Shore hardness | ShoreA,100°C,168hr,inIRM903Oil | ISO 1817 | -13 |
| Quality change rate | 23°C,168hr,inAceticAcid | ASTM D471 | 1.2 % |
| 23°C,168hr,inIsopropylAlcohol | ASTM D471 | -5.0 % | |
| 23°C,168hr,inMethylethylketone | ASTM D471 | -12 % | |
| 23°C,168hr,inSodiumChloride,15% | ASTM D471 | 0.10 % | |
| 23°C,168hr,inSodiumHydroxide,50% | ASTM D471 | 0.0 % | |
| 23.0°C,168hr,inSodiumHydroxide,50% | ISO 1817 | 0.0 % | |
| Shore hardness | ShoreA,125°C,168hr,inIRM903Oil | ISO 1817 | -15 |
| Quality change rate | 23°C,168hr,inCyclohexane | ASTM D471 | -3.4 % |
| 23°C,168hr,inEthanol,95% | ASTM D471 | -0.60 % | |
| 23°C,168hr,inEthanol,95% | ASTM D471 | -0.60 % | |
| 23°C,168hr,inHydrochloricAcid,10% | ASTM D471 | 0.10 % | |
| 23°C,168hr,inHydrochloricAcid,10% | ASTM D471 | 0.10 % | |
| 23.0°C,168hr,inSodiumChloride,15% | ISO 1817 | 0.10 % | |
| 23.0°C,168hr,inHydrochloricAcid,10% | ISO 1817 | 0.10 % | |
| 23.0°C,168hr,inSulfuricAcid,98% | ISO 1817 | 1.1 % | |
| 100°C,168hr,inDeionizedWater | ISO 1817 | 1.4 % | |
| 23.0°C,168hr,inAceticAcid | ISO 1817 | 1.2 % | |
| 100°C,168hr,inIRM903Oil | ISO 1817 | 35 % | |
| 125°C,168hr,inIRM903Oil | ISO 1817 | 44 % | |
| 125°C,168hr,inIRM903Oil | ISO 1817 | 44 % | |
| Volume change | 125°C,70hr,在IRM903油中 | ASTM D471 | 40 % |
| 125°C,70hr,在IRM903油中 | ASTM D471 | 40 % | |
| 125°C,70hr,在IRM903油中 | ISO 1817 | 40 % | |
| 125°C,70hr,在IRM903油中 | ISO 1817 | 40 % |
IMPORTANT NOTES: Plas.com collected the data in the data sheet from the material manufacturers. Plas.com makes the best effort to improve the accuracy of the data, but has no responsibility for the data. We strongly recommend verifying the validity of the data with the material manufacturers before making a final decision.