Material Description
- Material Properties:Filler: Glass fiber reinforced material|30% filler by weight
- Application Areas:--
- Color:--
- Grade:--
Technical Data Sheet
| impact performance | Test Condition | Test Method | Test Result |
|---|---|---|---|
| Impact strength of simply supported beam without notch | 23°C | ISO 179/1eU | 90 kJ/m² |
| -30°C | ISO 179/1eU | 75 kJ/m² |
| flammability | Test Condition | Test Method | Test Result |
|---|---|---|---|
| Burning wire flammability index | 2.0mm | IEC 60695-2-12 | 700 °C |
| UL flame retardant rating | 0.8mm | UL 94 | HB |
| Burning rate | FMVSS302 | 0.0 mm/min |
| mechanical properties | Test Condition | Test Method | Test Result |
|---|---|---|---|
| Tensile modulus | ISO 527-2/1A/1 | 9800 Mpa | |
| tensile strength | Break | ISO 527-2/1A/5 | 190 Mpa |
| Tensile strain | Break | ISO 527-2/1A/5 | 3.6 % |
| bending strength | ISO 178 | 290 Mpa | |
| Bending modulus | ISO 178 | 8900 Mpa |
| thermal performance | Test Condition | Test Method | Test Result |
|---|---|---|---|
| Melting temperature | ISO 11357 | 260 °C | |
| Vicat softening temperature | ISO 306/B50 | 250 °C | |
| Hot deformation temperature | 1.8MPa,Unannealed | ISO 75-2/Af | 245 °C |
| 0.45MPa,Unannealed | ISO 75-2/Bf | 255 °C |
| Physical properties | Test Condition | Test Method | Test Result |
|---|---|---|---|
| Water absorption rate | Equilibrium,23°C,2.00mm,50%RH | ISO 62 | 1.6 % |
| Saturation,23°C,2.00mm | ISO 62 | 6.2 % | |
| Shrinkage rate | MD | ISO 294-4 | 0.50 % |
| TD | ISO 294-4 | 1.2 % |
| Electrical performance | Test Condition | Test Method | Test Result |
|---|---|---|---|
| Compared to the anti leakage trace index | IEC 60112 | V | |
| Volume resistivity | IEC 60093 | 1E+15 ohms·cm | |
| Surface resistivity | IEC 60093 | 1E+12 ohms |
IMPORTANT NOTES: Plas.com collected the data in the data sheet from the material manufacturers. Plas.com makes the best effort to improve the accuracy of the data, but has no responsibility for the data. We strongly recommend verifying the validity of the data with the material manufacturers before making a final decision.