| mechanical properties | شرایط آزمون | روش آزمون | SABIC INNOVATIVE SHANGHAI/X4820 BK1006 |
|---|---|---|---|
| elongation | Break | ASTM D638 | 140 % |
| bending strength | ISO 178 | 87.0 Mpa | |
| Bending modulus | 50.0mmSpan | ASTM D790 | 2900 Mpa |
| Tensile modulus | ISO 527-2/1 | 3000 Mpa | |
| ASTM D638 | 3200 Mpa | ||
| tensile strength | Break | ISO 527-2/50 | 52.0 Mpa |
| Yield | ISO 527-2/50 | 58.0 Mpa | |
| Tensile strain | Break | ISO 527-2/50 | 100 % |
| bending strength | Yield,50.0mmSpan | ASTM D790 | 91.0 Mpa |
| tensile strength | Break | ASTM D638 | 58.0 Mpa |
| Yield | ASTM D638 | 57.0 Mpa | |
| Bending modulus | ISO 178 | 2850 Mpa | |
| elongation | Yield | ASTM D638 | 4.2 % |
| Tensile strain | Yield | ISO 527-2/50 | 4.2 % |
| thermal performance | شرایط آزمون | روش آزمون | SABIC INNOVATIVE SHANGHAI/X4820 BK1006 |
| Hot deformation temperature | 1.8MPa,Unannealed,3.20mm | ASTM D648 | 98.0 °C |
| 1.8MPa,Unannealed,64.0mmSpan | ISO 75-2/Af | 94.0 °C | |
| Vicat softening temperature | -- | ISO 306/B50 | 132 °C |
| Linear coefficient of thermal expansion | MD:-40to40°C | ISO 11359-2 | 7.5E-05 cm/cm/°C |
| MD:-40to40°C | ASTME831 | 7.5E-05 cm/cm/°C | |
| TD:-40to40°C | ASTME831 | 1.1E-04 cm/cm/°C | |
| Vicat softening temperature | ASTM D152510 | 130 °C | |
| -- | ISO 306/B120 | 134 °C | |
| Linear coefficient of thermal expansion | TD:-40to40°C | ISO 11359-2 | 1.1E-04 cm/cm/°C |
| impact performance | شرایط آزمون | روش آزمون | SABIC INNOVATIVE SHANGHAI/X4820 BK1006 |
| Impact strength of cantilever beam gap | 23°C | ISO 180/1A | 55 kJ/m² |
| Charpy Notched Impact Strength | 23°C | ISO 179/1eA | 60 kJ/m² |
| Dart impact | 23°C,TotalEnergy | ASTM D3763 | 60.0 J |
| Impact strength of cantilever beam gap | -30°C | ISO 180/1A | 15 kJ/m² |
| Physical properties | شرایط آزمون | روش آزمون | SABIC INNOVATIVE SHANGHAI/X4820 BK1006 |
| Melt Volume Flow Rate (MVR) | 265°C/5.0kg | ISO 1133 | 12.0 cm3/10min |
| Water absorption rate | Equilibrium,23°C,50%RH | ISO 62 | 0.14 % |
| Shrinkage rate | MD:3.20mm | Internal Method | 0.95-1.1 % |
| Water absorption rate | Saturation,23°C | ISO 62 | 0.42 % |
| melt mass-flow rate | 250°C/5.0kg | ASTM D1238 | 10 g/10min |