PPA AE-4133 NT SOLVAY USA
133
Form:Granules | Grade:Injection grade
Properties:
High temperature resistanLow moisture absorptionhigh strengthFiller: Glass fiber reinfFiller by weight
Typical Applications:
Office suppliesLaptop caseElectrical componentsElectrical/Electronic ApplicationsVehicle electronics
Product Description
Certificates(0)
Datasheet
Product Description
| Typical Applications: | Office supplies | Laptop case | Electrical components | Electrical/Electronic Applications | Vehicle electronics |
| Properties: | High temperature resistan | Low moisture absorption | high strength | Filler: Glass fiber reinf | Filler by weight |
Certificates
No Data...
Technical Data Sheet
| impact performance | Test Condition | Test Method | Test Result | Test Unit |
|---|---|---|---|---|
| Impact strength of simply supported beam without notch | 23°C | ISO 179/1eU | 79 | kJ/m² |
| Suspended wall beam without notch impact strength | 23°C | ISO 180/1U | 68 | kJ/m² |
| flammability | Test Condition | Test Method | Test Result | Test Unit |
| UL flame retardant rating | 3.2mm | UL 94 | HB | |
| mechanical properties | Test Condition | Test Method | Test Result | Test Unit |
| Tensile modulus | 23°C | ISO 527-2 | 12000 | Mpa |
| tensile strength | Break,23°C | ISO 527-2 | 210 | Mpa |
| Tensile strain | Break,23°C | ISO 527-2 | 2.5 | % |
| Bending modulus | 23°C | ISO 178 | 10700 | Mpa |
| bending strength | 23°C | ISO 178 | 295 | Mpa |
| Bending strain | ISO 178 | 3.1 | % | |
| thermal performance | Test Condition | Test Method | Test Result | Test Unit |
| Melting temperature | ISO 11357-3 | 327 | °C | |
| Linear coefficient of thermal expansion | MD:0to100°C | ASTME831 | 2E-05 | cm/cm/°C |
| MD:100to200°C | ASTME831 | 1.5E-05 | cm/cm/°C | |
| TD:0to100°C | ASTME831 | 7.6E-05 | cm/cm/°C | |
| TD:100to200°C | ASTME831 | 1.2E-04 | cm/cm/°C | |
| Hot deformation temperature | 1.8MPa,Unannealed | ISO 75-2/A | >300 | °C |
| Glass transition temperature | DSC | 95.0 | °C | |
| Physical properties | Test Condition | Test Method | Test Result | Test Unit |
| Shrinkage rate | MD | ASTM D955 | 0.40 | % |
| TD | ASTM D955 | 0.80 | % | |
| Water absorption rate | 24hr | ASTM D570 | 0.23 | % |
| Electrical performance | Test Condition | Test Method | Test Result | Test Unit |
| Dissipation factor | 1MHz | ASTM D150 | 0.015 | |
| Volume resistivity | ASTM D257 | 5.6E+15 | ohms·cm | |
| Dielectric strength | 3.20mm | ASTM D149 | 19 | KV/mm |
| Dielectric constant | 60Hz | ASTM D150 | 4.10 | |
| 1MHz | ASTM D150 | 3.75 | ||
| Dissipation factor | 60Hz | ASTM D150 | 6E-03 |
IMPORTANT NOTES: Plas.com collected the data in the data sheet from the material manufacturers. Plas.com makes the best effort to improve the accuracy of the data, but has no responsibility for the data. We strongly recommend verifying the validity of the data with the material manufacturers before making a final decision.