PC PC-122 TAIWAN CHIMEI
581
Form:Granules
Properties:
transparentHigh mobility
Typical Applications:
containerchip
Product Description
Certificates(3)
Datasheet
Product Description
| Typical Applications: | container | chip |
| Properties: | transparent | High mobility |
Certificates



Technical Data Sheet
| impact performance | Test Condition | Test Method | Test Result | Test Unit |
|---|---|---|---|---|
| Impact strength of cantilever beam gap | 23°C,3.20mm | ASTM D256 | 820 | J/m |
| 23°C | ISO 180/4A | 60 | kJ/m² | |
| Charpy Notched Impact Strength | 23°C | ISO 179 | 60 | kJ/m² |
| flammability | Test Condition | Test Method | Test Result | Test Unit |
| UL flame retardant rating | 3.2mm | UL 94 | V-2 | |
| 0.38mm | UL 94 | V-2 | ||
| mechanical properties | Test Condition | Test Method | Test Result | Test Unit |
| bending strength | ISO 178 | 90.0 | Mpa | |
| ASTM D790 | 89.8 | Mpa | ||
| Bending modulus | ISO 178 | 2400 | Mpa | |
| ASTM D790 | 2340 | Mpa | ||
| Tensile strain | Break | ISO 527-2/50 | 120 | % |
| elongation | Break | ASTM D638 | 110 | % |
| tensile strength | Break | ISO 527-2/50 | 70.0 | Mpa |
| Yield | ISO 527-2/50 | 63.0 | Mpa | |
| Yield | ASTM D638 | 61.6 | Mpa | |
| thermal performance | Test Condition | Test Method | Test Result | Test Unit |
| Linear coefficient of thermal expansion | MD | ISO 11359-2 | 6.0E-5to8.0E-5 | cm/cm/°C |
| Vicat softening temperature | -- | ISO 306/B50 | 145 | °C |
| -- | ISO 306/A50 | 150 | °C | |
| ASTM D15257 | 150 | °C | ||
| Hot deformation temperature | 1.8MPa,Annealed | ISO 75-2/A | 143 | °C |
| 1.8MPa,Unannealed | ISO 75-2/A | 128 | °C | |
| 0.45MPa,Annealed | ASTM D648 | 144 | °C | |
| Physical properties | Test Condition | Test Method | Test Result | Test Unit |
| Shrinkage rate | ISO 294-4 | 0.50-0.70 | % | |
| Melt Volume Flow Rate (MVR) | 300°C/1.2kg | ISO 1133 | 22.0 | cm3/10min |
| melt mass-flow rate | 300°C/1.2kg | ASTM D1238 | 22 | g/10min |
| density | 23°C | ISO 1183 | 1.20 | g/cm³ |
| 比重 | ASTM D792 | 1.20 | g/cm³ | |
| hardness | Test Condition | Test Method | Test Result | Test Unit |
| Rockwell hardness | M-Scale | ASTM D785 | 77 |
IMPORTANT NOTES: Plas.com collected the data in the data sheet from the material manufacturers. Plas.com makes the best effort to improve the accuracy of the data, but has no responsibility for the data. We strongly recommend verifying the validity of the data with the material manufacturers before making a final decision.