PET UmaPET LO/LI Ester Industries Ltd.
Product Description
Certificates(0)
Datasheet
Product Description
Certificates
No Data...
Technical Data Sheet
| optical performance | Test Condition | Test Method | Test Result | Test Unit |
|---|---|---|---|---|
| turbidity | 12.0μm | ASTM D1003 | 3.5 | % |
| 10.0μm | ASTM D1003 | 3.5 | % | |
| 15.0μm | ASTM D1003 | 3.5 | % | |
| 23.0μm | ASTM D1003 | 4.5 | % | |
| mechanical properties | Test Condition | Test Method | Test Result | Test Unit |
| Friction coefficient | Itself - Dynamic1 | ASTM D1894 | 0.50 | |
| Itself - Dynamic2 | ASTM D1894 | 0.50 | ||
| Itself - Dynamic3 | ASTM D1894 | 0.50 | ||
| Itself - Dynamic4 | ASTM D1894 | 0.42 | ||
| Itself - Static5 | ASTM D1894 | 0.45 | ||
| Itself - Static6 | ASTM D1894 | 0.45 | ||
| Itself - Static7 | ASTM D1894 | 0.45 | ||
| Itself - Static8 | ASTM D1894 | 0.48 | ||
| Physical properties | Test Condition | Test Method | Test Result | Test Unit |
| Shrinkage rate | MD:150°C,30分钟,0.0150mm | ASTM D1204 | 2.5 | % |
| MD:150°C,30分钟,0.0230mm | ASTM D1204 | 2.5 | % | |
| TD:150°C,30分钟,0.0100mm | ASTM D1204 | 0.40 | % | |
| TD:150°C,30分钟,0.0120mm | ASTM D1204 | 0.40 | % | |
| TD:150°C,30分钟,0.0150mm | ASTM D1204 | 0.40 | % | |
| TD:150°C,30分钟,0.0230mm | ASTM D1204 | 0.40 | % | |
| MD:150°C,30分钟,0.0100mm | ASTM D1204 | 2.5 | % | |
| MD:150°C,30分钟,0.0120mm | ASTM D1204 | 2.5 | % | |
| film | Test Condition | Test Method | Test Result | Test Unit |
| consumption | 15.0μm | Internal Method | 47.6 | m²/kg |
| 23.0μm | Internal Method | 31.0 | m²/kg | |
| film thickness | 10121523 | µm | ||
| 10.12.15.23µm | ||||
| tensile strength | MD:Break,10μm | ASTM D882 | 206 | MPa |
| elongation | MD:Break,23μm | ASTM D882 | 100 | % |
| TD:Break,10μm | ASTM D882 | 90 | % | |
| TD:Break,12μm | ASTM D882 | 90 | % | |
| TD:Break,15μm | ASTM D882 | 90 | % | |
| TD:Break,23μm | ASTM D882 | 90 | % | |
| consumption | 10.0μm | Internal Method | 71.4 | m²/kg |
| 12.0μm | Internal Method | 59.5 | m²/kg | |
| tensile strength | MD:Break,12μm | ASTM D882 | 206 | MPa |
| MD:Break,15μm | ASTM D882 | 186 | MPa | |
| MD:Break,23μm | ASTM D882 | 186 | MPa | |
| TD:Break,10μm | ASTM D882 | 216 | MPa | |
| TD:Break,12μm | ASTM D882 | 216 | MPa | |
| TD:Break,15μm | ASTM D882 | 206 | MPa | |
| TD:Break,23μm | ASTM D882 | 206 | MPa | |
| elongation | MD:Break,10μm | ASTM D882 | 100 | % |
| MD:Break,12μm | ASTM D882 | 100 | % | |
| MD:Break,15μm | ASTM D882 | 100 | % | |
| Supplementary Information | Test Condition | Test Method | Test Result | Test Unit |
| wetting tension | Plainside:23.0μm | ASTM D2578 | 42 | dyne/cm |
| Coatedside:10.0μm | ASTM D2578 | 48 | dyne/cm | |
| Coatedside:12.0μm | ASTM D2578 | 48 | dyne/cm | |
| Coatedside:15.0μm | ASTM D2578 | 48 | dyne/cm | |
| Coatedside:23.0μm | ASTM D2578 | 48 | dyne/cm | |
| Plainside:10.0μm | ASTM D2578 | 42 | dyne/cm | |
| Plainside:12.0μm | ASTM D2578 | 42 | dyne/cm | |
| Plainside:15.0μm | ASTM D2578 | 42 | dyne/cm |
IMPORTANT NOTES: Plas.com collected the data in the data sheet from the material manufacturers. Plas.com makes the best effort to improve the accuracy of the data, but has no responsibility for the data. We strongly recommend verifying the validity of the data with the material manufacturers before making a final decision.