PPO/PA GTX8430-1710 SABIC INNOVATIVE US
190
Form:Granules | Grade:Injection grade
Properties:
Hydrolysis resistanceHigh temperature resistanDimensional stabilityHigh mobilityFiller: Glass fiber reinf40%Filler by weight
Typical Applications:
Electrical applicationsIndustrial machineryParts under the hood of a car
Product Description
Certificates(0)
Datasheet
Product Description
| Typical Applications: | Electrical applications | Industrial machinery | Parts under the hood of a car |
| Properties: | Hydrolysis resistance | High temperature resistan | Dimensional stability | High mobility | Filler: Glass fiber reinf | 40% | Filler by weight |
Certificates
No Data...
Technical Data Sheet
| mechanical properties | Test Condition | Test Method | Test Result | Test Unit |
|---|---|---|---|---|
| bending strength | Yield,50.0mmSpan4 | ASTM D790 | 249 | Mpa |
| --5,6 | ISO 178 | 280 | Mpa | |
| Bending modulus | --5 | ISO 178 | 12300 | Mpa |
| 50.0mmSpan4 | ASTM D790 | 11900 | Mpa | |
| elongation | Break | ISO 527-2/5 | 2.0 | % |
| Break3 | ASTM D638 | 2.0 | % | |
| tensile strength | Break | ISO 527-2/5 | 198 | Mpa |
| Break3 | ASTM D638 | 178 | Mpa | |
| Tensile modulus | -- | ISO 527-2/1 | 13900 | Mpa |
| --2 | ASTM D638 | 13500 | Mpa | |
| thermal performance | Test Condition | Test Method | Test Result | Test Unit |
| Vicat softening temperature | ISO 306/B50 | 246 | °C | |
| Hot deformation temperature | 1.8MPa,Unannealed,64.0mmSpan9 | ISO 75-2/Af | 244 | °C |
| 1.8MPa,Unannealed,6.40mm | ASTM D648 | 247 | °C | |
| 0.45MPa,Unannealed,64.0mmSpan9 | ISO 75-2/Bf | 258 | °C | |
| 0.45MPa,Unannealed,6.40mm | ASTM D648 | 260 | °C | |
| Linear coefficient of thermal expansion | TD:-40to40°C | ASTME831 | 9.0E-5到9.4E-5 | cm/cm/°C |
| MD:-40to40°C | ASTME831 | 1.6E-5到2.0E-5 | cm/cm/°C | |
| Physical properties | Test Condition | Test Method | Test Result | Test Unit |
| Water absorption rate | Equilibrium,23°C,50%RH | ISO 62 | 0.10 | % |
| Equilibrium,23°C | ASTM D570 | 0.30 | % | |
| Shrinkage rate | TD:3.20mm | Internal Method | 0.60-0.63 | % |
| MD:3.20mm | Internal Method | 0.24-0.27 | % | |
| Melt Volume Flow Rate (MVR) | 220°C/5.0kg | ISO 1133 | 10.0 | cm3/10min |
| hardness | Test Condition | Test Method | Test Result | Test Unit |
| Rockwell hardness | R-Scale | ASTM D785 | 108 |
IMPORTANT NOTES: Plas.com collected the data in the data sheet from the material manufacturers. Plas.com makes the best effort to improve the accuracy of the data, but has no responsibility for the data. We strongly recommend verifying the validity of the data with the material manufacturers before making a final decision.