PC/ABS FXE1414L-955 SABIC INNOVATIVE NANSHA
74
Form:Granules | Grade:Injection grade
Properties:
Low temperature resistanctransparentFlame retardant
Typical Applications:
Household appliancesElectrical appliancesElectronic fieldElectrical field
Product Description
Certificates(0)
Datasheet
Product Description
| Typical Applications: | Household appliances | Electrical appliances | Electronic field | Electrical field |
| Properties: | Low temperature resistanc | transparent | Flame retardant |
Certificates
No Data...
Technical Data Sheet
| impact performance | Test Condition | Test Method | Test Result | Test Unit |
|---|---|---|---|---|
| Dart impact | 23°C, Total Energy | ASTM D3763 | 68.0 | J |
| flammability | Test Condition | Test Method | Test Result | Test Unit |
| UL flame retardant rating | 0.40 mm | UL 94 | HB | |
| mechanical properties | Test Condition | Test Method | Test Result | Test Unit |
| Tensile modulus | --2 | ASTM D638 | 2030 | Mpa |
| -- | ISO 527-2/1 | 2000 | Mpa | |
| tensile strength | Yield3 | ASTM D638 | 52.0 | Mpa |
| Yield | ISO 527-2/50 | 52.0 | Mpa | |
| Break3 | ASTM D638 | 54.0 | Mpa | |
| Break | ISO 527-2/50 | 47.0 | Mpa | |
| elongation | Yield3 | ASTM D638 | 5.0 | % |
| Yield | ISO 527-2/50 | 5.0 | % | |
| Break3 | ASTM D638 | 84 | % | |
| Break | ISO 527-2/50 | 75 | % | |
| Bending modulus | 50.0 mm Span4 | ASTM D790 | 2050 | Mpa |
| --5 | ISO 178 | 2110 | Mpa | |
| bending strength | --5,6 | ISO 178 | 83.0 | Mpa |
| Yield, 50.0 mm Span4 | ASTM D790 | 86.0 | Mpa | |
| injection | Test Condition | Test Method | Test Result | Test Unit |
| drying temperature | 120 | °C | ||
| drying time | 3.0 to 4.0 | hr | ||
| Suggested maximum moisture content | 0.020 | % | ||
| Hopper temperature | 60 to 80 | °C | ||
| Temperature at the rear of the barrel | 260 to 280 | °C | ||
| Temperature in the middle of the barrel | 280 to 305 | °C | ||
| Temperature at the front of the material cylinder | 295 to 315 | °C | ||
| Spray nozzle temperature | 290 to 310 | °C | ||
| Processing (melt) temperature | 295 to 315 | °C | ||
| Mold temperature | 70 to 95 | °C | ||
| thermal performance | Test Condition | Test Method | Test Result | Test Unit |
| Hot deformation temperature | 1.8 MPa, Unannealed, 3.20 mm | ASTM D648 | 121 | °C |
| 1.8 MPa, Unannealed, 4.00 mm, 64.0 mm Span8 | ISO 75-2/Af | 118 | °C | |
| Vicat softening temperature | -- | ASTM D15259 | 138 | °C |
| -- | ISO 306/B120 | 146 | °C | |
| Linear coefficient of thermal expansion | Flow : -40 to 40°C | ASTM E831 | 7.0E-5 | cm/cm/°C |
| Across Flow : -40 to 40°C | ASTM E831 | 6.7E-5 | cm/cm/°C | |
| Across Flow : -40°C | ISO 11359-2 | 8.2E-5 | cm/cm/°C | |
| Physical properties | Test Condition | Test Method | Test Result | Test Unit |
| melt mass-flow rate | 300°C/1.2 kg | ASTM D1238 | 11 | g/10 min |
| Melt Volume Flow Rate (MVR) | 300°C/1.2 kg | ISO 1133 | 10.0 | cm3/10min |
| Shrinkage rate | 3.20 mm,Flow | Internal Method | 0.40 - 0.80 | % |
| Water absorption rate | Saturation, 23°C | ISO 62 | 0.17 | % |
| Equilibrium, 23°C, 50% RH | ISO 62 | 0.070 | % |
IMPORTANT NOTES: Plas.com collected the data in the data sheet from the material manufacturers. Plas.com makes the best effort to improve the accuracy of the data, but has no responsibility for the data. We strongly recommend verifying the validity of the data with the material manufacturers before making a final decision.