PPS SUSTEEL® GM-70 TOSOH JAPAN
27
- Properties:High temperature resistancurrencystandard
- Usages:Electrical fieldElectronic fieldHousehold appliancesHousehold appliancesFlame retardant insulationBottle capCasters
- Certificates:UL
Technical Data Sheet
| machinability | Test Condition | Test Method | Test Result |
|---|---|---|---|
| Shrinkage rate | 机械方向 | ASTM D-955 | 0.3 % |
| Across Flow | ASTM D-955 | 0.6 % |
| mechanical properties | Test Condition | Test Method | Test Result |
|---|---|---|---|
| Impact strength of cantilever beam gap | Notched | ASTM D-256 | 59(6) J/m(kg.cm/cm) |
| Unnotched | ASTM D-256 | 137(14) J/m(kg.cm/cm) | |
| tensile strength | ASTM D-638 | 108(1100) MPa(Kg/cm2) | |
| Rockwell hardness | ASTM D-785 | 122 Rscal | |
| bending strength | ASTM D-790 | 206(2100) MPa(Kg/cm2) | |
| Tensile modulus | ASTM D-790 | 21(2.1) | |
| elongation | ASTM D-638 | 0.4 % |
| thermal performance | Test Condition | Test Method | Test Result |
|---|---|---|---|
| Linear coefficient of thermal expansion | Tosoh Method | 2.6 | |
| 0.51(0.44) W/M.K(kcal/m.hr.℃) | |||
| Hot deformation temperature | 18.6kg/cm2 | ASTM D-648 | >260 °C |
| Electrical performance | Test Condition | Test Method | Test Result |
|---|---|---|---|
| Volume resistivity | ASTM D-257 | 1×1016 Ω.cm | |
| Dielectric constant | 1MHz | ASTM D-150 | 5.4 |
| Dissipation factor | 1MHz | ASTM D-150 | 0.0015 |
| Dielectric strength | ASTM D-149 | 12 KV/mm |
IMPORTANT NOTES: Plas.com collected the data in the data sheet from the material manufacturers. Plas.com makes the best effort to improve the accuracy of the data, but has no responsibility for the data. We strongly recommend verifying the validity of the data with the material manufacturers before making a final decision.