plas
Log In

TPV Supersoft Actymer® AE-2010S RIKEN JAPAN

0

Technical Data Sheet

elastomerTest ConditionTest MethodTest Result
tensile strength100%StrainISO 370.300 MPa
tensile strengthYieldISO 373.50 MPa
elongationBreakISO 37950 %
tear strengthISO 34-113 kN/m
Permanent compression deformation70°C,72hrISO 81530 %
Permanent compression deformation120°C,72hrISO 81571 %
thermal performanceTest ConditionTest MethodTest Result
Brittle temperatureISO 974-60.0 °C
Physical propertiesTest ConditionTest MethodTest Result
densityISO 11830.918 g/cm³
hardnessTest ConditionTest MethodTest Result
Shore hardnessShoreA,15SecISO 86810
agingTest ConditionTest MethodTest Result
Change rate of tensile strength in air136°C,168hrISO 188-7.0 %
Tensile stress change rate136°C,168hr,BreakISO 188-15 %
IMPORTANT NOTES: Plas.com collected the data in the data sheet from the material manufacturers. Plas.com makes the best effort to improve the accuracy of the data, but has no responsibility for the data. We strongly recommend verifying the validity of the data with the material manufacturers before making a final decision.