POM TE-01 KAIFENG LONGYU
37
Form:Granules | Grade:Injection grade
Properties:
High toughnessCold resistanceTougheningcurrencyHigh toughnessCold resistanceHas high notch impact str
Typical Applications:
Electrical fieldElectronic field
Product Description
Certificates(0)
Datasheet
Product Description
| Typical Applications: | Electrical field | Electronic field |
| Properties: | High toughness | Cold resistance | Toughening | currency | High toughness | Cold resistance | Has high notch impact str |
Certificates
No Data...
Technical Data Sheet
| Basic performance | Test Condition | Test Method | Test Result | Test Unit |
|---|---|---|---|---|
| water content | 0.090 | % | ||
| mechanical properties | Test Condition | Test Method | Test Result | Test Unit |
| Impact strength of cantilever beam gap | ISO 179-1 | 9.65 | kJ/m² | |
| bending strength | ISO 178 | 58.60 | Mpa | |
| tensile strength | ISO 527-1.2 | 47.96 | Mpa | |
| bending strength | ISO 178 | 69.8 | Mpa | |
| tensile strength | ISO 527-1.2 | 49.4 | Mpa | |
| Elongation at Break | ISO 527-1.2 | 65.8 | % | |
| Impact strength of cantilever beam gap | ISO 179-1 | 11.4 | kJ/㎡ | |
| Physical properties | Test Condition | Test Method | Test Result | Test Unit |
| melt mass-flow rate | ISO 1133 | 2.41 | g/10min |
IMPORTANT NOTES: Plas.com collected the data in the data sheet from the material manufacturers. Plas.com makes the best effort to improve the accuracy of the data, but has no responsibility for the data. We strongly recommend verifying the validity of the data with the material manufacturers before making a final decision.