Material Comparison
Product Info
Product Name
Brand Name
Usages
Properties
Certificates

PA66 CM3001G-45 BK TORAY JAPAN
Amilan®
OA device,electrical equipment
Glass fiber reinforced
--
--
--
--
--
--
--
--
--
--
--
--
--
--
--
Plastic Datasheets
| hardness | Test Condition | Test Method | TORAY JAPAN/CM3001G-45 BK |
|---|---|---|---|
| Rockwell hardness | R -Sale, 80°C | ISO 2039-2 | 24 |
| M -Sale, 23°C | ISO 2039-2 | 97 | |
| R -Sale, 23°C | ISO 2039-2 | 121 |
| thermal performance | Test Condition | Test Method | TORAY JAPAN/CM3001G-45 BK |
|---|---|---|---|
| Hot deformation temperature | 0.45 MPa, Unannealed | ISO 75-2/B | 262 °C |
| Linear coefficient of thermal expansion | Flow | ISO 11359-2 | 2.0E-5 - 3.0E-5 cm/cm/°C |
| Melting temperature | DSC | 265 °C | |
| specific heat | 1800 J/kg/°C | ||
| thermal conductivity | 0.40 W/m/K |
| mechanical properties | Test Condition | Test Method | TORAY JAPAN/CM3001G-45 BK |
|---|---|---|---|
| Bending modulus | 80°C | ISO 178 | 5800 Mpa |
| -40°C | ISO 178 | 11600 Mpa | |
| 23°C | ISO 178 | 9500 Mpa | |
| bending strength | 80°C | ISO 178 | 190 Mpa |
| 23°C | ISO 178 | 290 Mpa | |
| -40°C | ISO 178 | 325 Mpa | |
| Compressive stress | -40°C | ISO 604 | 250 Mpa |
| 80°C | ISO 604 | 110 Mpa | |
| 23°C | ISO 604 | 180 Mpa | |
| Friction coefficient - vs. Metal | Suzuki Method | 0.15 | |
| shear strength | 23°C | ASTM D732 | 95.0 Mpa |
| Taber abraser | 1000 Cycles | ISO 9352 | 0.400 mg |
| Tensile strain | Break, -40°C | ISO 527-2 | 2.0 % |
| Break, 80°C | ISO 527-2 | 5.0 % | |
| Break, 23°C | ISO 527-2 | 2.5 % | |
| tensile strength | 80°C | ISO 527-2 | 120 Mpa |
| -40°C | ISO 527-2 | 235 Mpa | |
| 23°C | ISO 527-2 | 190 Mpa |
| Electrical performance | Test Condition | Test Method | TORAY JAPAN/CM3001G-45 BK |
|---|---|---|---|
| Arc resistance | UL 746 | 114 sec | |
| Dielectric constant | 23°C, 1 kHz | IEC 60250 | 4.40 |
| 23°C, 50 Hz | IEC 60250 | 4.60 | |
| 23°C, 1 MHz | IEC 60250 | 3.90 | |
| Dielectric strength | IEC 60243-1 | 20 KV/mm | |
| Dissipation factor | 23°C, 50 Hz | IEC 60250 | 0.020 |
| 23°C, 1 MHz | IEC 60250 | 0.020 | |
| 23°C, 1 kHz | IEC 60250 | 0.020 | |
| Volume resistivity | IEC 60093 | 1.0E+13 ohms·cm |
| Physical properties | Test Condition | Test Method | TORAY JAPAN/CM3001G-45 BK |
|---|---|---|---|
| density | 23°C | ISO 1183 | 1.37 g/cm³ |
| Shrinkage rate | 横向Flow : 3.00 mm | Internal Method | 0.60 - 0.90 % |
| Flow : 3.00 mm | Internal Method | 0.20 - 0.50 % | |
| Water absorption rate | 24 hr, 23°C | ISO 62 | 0.60 % |
| Saturation, 23°C | ISO 62 | 5.5 % |
| impact performance | Test Condition | Test Method | TORAY JAPAN/CM3001G-45 BK |
|---|---|---|---|
| Charpy Notched Impact Strength | -40°C | ISO 179 | 10 kJ/m² |
| 23°C | ISO 179 | 13 kJ/m² | |
| Impact strength of simply supported beam without notch | -40°C | ISO 179 | 60 kJ/m² |
| 23°C | ISO 179 | 65 kJ/m² |
| flammability | Test Condition | Test Method | TORAY JAPAN/CM3001G-45 BK |
|---|---|---|---|
| UL flame retardant rating | 0.79 mm | UL 94 | HB |