Impact resistance | Test Condition | Test Method | BASF GERMANY/2822HD |
---|---|---|---|
Impact strength of simply supported beam without notch | -30°C | ISO 179 | 80 kJ/m² |
23°C | ISO 179 | 120 kJ/m² |
hardness | Test Condition | Test Method | BASF GERMANY/2822HD |
---|---|---|---|
ball-indentation hardness | ISO 2039-1 | 70.0 Mpa |
Mechanical properties | Test Condition | Test Method | BASF GERMANY/2822HD |
---|---|---|---|
Tensile modulus | ISO 527-2 | 2000 Mpa | |
bending strength | ISO 178 | 70.0 Mpa | |
tensile strength | 屈服,23°C | ISO 527-2 | 48.0 Mpa |
Tensile creep modulus | 1000hr | ISO 899-1 | 1250 Mpa |
Tensile strain | 屈服,23°C | ISO 527-2 | 4.0 % |
Nominal tensile fracture strain | 23°C | ISO 527-2 | 12 % |
Electrical performance | Test Condition | Test Method | BASF GERMANY/2822HD |
---|---|---|---|
dielectric constant | 100Hz | IEC 60250 | 2.90 |
Volume resistivity | IEC 60093 | 1E+15 ohms·cm | |
Dissipation Factor | 100Hz | IEC 60250 | 0.016 |
Surface Resistivity | IEC 60093 | 1E+15 ohms | |
Dissipation Factor | 1MHz | IEC 60250 | 0.014 |
optical performance | Test Condition | Test Method | BASF GERMANY/2822HD |
---|---|---|---|
refractive index | ISO 489 | 1.540 |
physical property | Test Condition | Test Method | BASF GERMANY/2822HD |
---|---|---|---|
Apparent density | 0.59 g/cm³ | ||
Melt volume flow rate | 220°C/21.6kg | ISO 1133 | 17.0 cm3/10min |
Shrinkage rate | ISO 294-4 | 0.40-0.70 % | |
Water absorption rate | 饱和,23°C | ISO 62 | 0.70 % |
Melt volume flow rate | 220°C/10.0kg | ISO 1133 | 2.00 cm3/10min |
Thermal performance | Test Condition | Test Method | BASF GERMANY/2822HD |
---|---|---|---|
thermal conductivity | DIN 52612 | 0.17 W/m/K | |
Heat distortion temperature | 1.8MPa,Annealed,HDT | ISO 75-2/A | 90.0 °C |
vicat | -- | ISO 306/A50 | 105 °C |
-- | ISO 306/B50 | 93.0 °C | |
Linear coefficient of thermal expansion | MD | ISO 11359-2 | 8.0E-5to1.1E-4 cm/cm/°C |
Heat distortion temperature | 0.45MPa,Annealed,HDT | ISO 75-2/B | 94.0 °C |