Material Comparison
Add Comparison Model
Select Products for Comparison (1/4)
Highlight Differences
Hide Same
Product Name / Manufacturer / Model
Grade
Reference Price
| mechanical properties | Test Condition | Test Method | SOLVAY USA/AT-6130 HS |
|---|---|---|---|
| bending strength | ISO 178 | 225 Mpa | |
| elongation | Break | ASTM D638 | 3.2 % |
| bending strength | Yield | ASTM D790 | 236 Mpa |
| tensile strength | Break | ASTM D638 | 167 Mpa |
| Bending modulus | ASTM D790 | 7860 Mpa | |
| Tensile strain | Break | ISO 527-2 | 3.3 % |
| Bending modulus | ISO 178 | 7580 Mpa | |
| tensile strength | Break | ISO 527-2 | 170 Mpa |
| Tensile modulus | ISO 527-2 | 9310 Mpa | |
| Physical properties | Test Condition | Test Method | SOLVAY USA/AT-6130 HS |
| Shrinkage rate | TD | ASTM D955 | 0.80 % |
| Water absorption rate | 24hr | ASTM D570 | 0.15 % |
| Shrinkage rate | MD | ASTM D955 | 0.50 % |
| density | ISO 1183/A | 1.34 g/cm³ | |
| thermal performance | Test Condition | Test Method | SOLVAY USA/AT-6130 HS |
| Hot deformation temperature | 0.45MPa,Unannealed | ISO 75-2/B | 298 °C |
| 1.8MPa,Unannealed | ISO 75-2/A | 276 °C | |
| Melting temperature | ASTM D3418 | 306 °C | |
| ISO 11357-3 | 310 °C | ||
| impact performance | Test Condition | Test Method | SOLVAY USA/AT-6130 HS |
| Impact strength of cantilever beam gap | ASTM D256 | 130 J/m | |
| Charpy Notched Impact Strength | ISO 179/1eA | 13 kJ/m² |