| mechanical properties | Test Condition | Test Method | A SCHULMAN USA/PCR GF 30 BK |
|---|---|---|---|
| Tensile modulus | ISO 527-2/1A/1 | 11000 Mpa | |
| tensile strength | Break | ISO 527-2/1A/5 | 142 Mpa |
| Tensile strain | Break | ISO 527-2/1A/5 | 2.1 % |
| flammability | Test Condition | Test Method | A SCHULMAN USA/PCR GF 30 BK |
| UL flame retardant rating | 3.0mm | IEC 60695-11-10,-20 | HB |
| Burning wire flammability index | 1.5mm | IEC 60695-2-12 | 700 °C |
| UL flame retardant rating | 1.5mm | IEC 60695-11-10,-20 | HB |
| Burning wire flammability index | 3.0mm | IEC 60695-2-12 | 800 °C |
| Extreme Oxygen Index | ISO 4589-2 | 19 % | |
| Hot filament ignition temperature | 1.5mm | IEC 60695-2-13 | 725 °C |
| 3.0mm | IEC 60695-2-13 | 825 °C | |
| Burning rate | ISO 3795 | 26 mm/min | |
| thermal performance | Test Condition | Test Method | A SCHULMAN USA/PCR GF 30 BK |
| Vicat softening temperature | -- | ISO 306/B50 | 204 °C |
| Ball Pressure Test | 200°C | IEC 60695-10-2 | Pass |
| Hot deformation temperature | 1.8MPa,Unannealed | ISO 75-2/Af | 205 °C |
| Vicat softening temperature | -- | ISO 306/A50 | 218 °C |
| Hot deformation temperature | 0.45MPa,Unannealed | ISO 75-2/Bf | 225 °C |
| Electrical performance | Test Condition | Test Method | A SCHULMAN USA/PCR GF 30 BK |
| Volume resistivity | IEC 60093 | >1.0E+12 ohms·cm | |
| Surface resistivity | IEC 60093 | >1.0E+16 ohms | |
| Physical properties | Test Condition | Test Method | A SCHULMAN USA/PCR GF 30 BK |
| Water absorption rate | 23°C,24hr | ISO 62 | 0.30 % |
| Melt Volume Flow Rate (MVR) | 260°C/2.16kg | ISO 1133 | 20.0 cm3/10min |
| hardness | Test Condition | Test Method | A SCHULMAN USA/PCR GF 30 BK |
| Ball Pressure Test | H358/30 | ISO 2039-1 | 263 Mpa |
| impact performance | Test Condition | Test Method | A SCHULMAN USA/PCR GF 30 BK |
| Impact strength of simply supported beam without notch | 23°C | ISO 179/1eU | 55 kJ/m² |
| -30°C | ISO 179/1eU | 50 kJ/m² |