Material Comparison
Product Info
Product Name
Brand Name
Usages
Properties
Certificates

TPV 4775B42 TEKNOR APEX BELGIUM
SARLINK®
--
--
--
--
--
--
--
--
--
--
--
--
--
--
--
--
--
Plastic Datasheets
hardness | Test Condition | Test Method | TEKNOR APEX BELGIUM/4775B42 |
---|---|---|---|
Shore hardness | 邵氏A,5秒,注塑 | ISO 868 | 76 |
邵氏A,5秒,挤塑 | ASTM D2240 | 74 | |
邵氏A,5秒,挤塑 | ISO 868 | 74 | |
邵氏A,5秒,注塑 | ASTM D2240 | 76 |
Supplementary Information | Test Condition | Test Method | TEKNOR APEX BELGIUM/4775B42 |
---|---|---|---|
Apparent viscosity | 200°C,剪切,毛细管法, @206/s | ASTM D3835 | 200 Pa·s |
200°C,剪切,毛细管法, @206/s | ISO 11443 | 200 |
elastomer | Test Condition | Test Method | TEKNOR APEX BELGIUM/4775B42 |
---|---|---|---|
elongation | 断裂 | ASTM D412 | 470 % |
compression set | 23°C,22hr | ISO 815 | 24 % |
70°C,22hr | ASTM D395 | 39 % | |
125°C,70hr | ASTM D395 | 56 % | |
elongation | 断裂 | ISO 37 | 470 % |
compression set | 125°C,70hr | ISO 815 | 56 % |
tensile strength | 流量:断裂 | ASTM D412 | 5.80 Mpa |
断裂 | ISO 37 | 6.30 Mpa | |
横向流量:100%应变 | ASTM D412 | 3.20 Mpa | |
compression set | 23°C,22hr | ASTM D395 | 24 % |
elongation | 流量:断裂 | ISO 37 | 410 % |
tensile strength | 流量:100%应变 | ISO 37 | 3.40 Mpa |
流量:断裂 | ISO 37 | 5.80 Mpa | |
compression set | 70°C,22hr | ISO 815 | 39 % |
elongation | 流量:断裂 | ASTM D412 | 410 % |
tear strength | 横向流量 | ASTM D624 | 31.5 kN/m |
横向流量 | ISO 34-1 | 31 kN/m | |
tensile strength | 断裂 | ASTM D412 | 6.30 Mpa |
横向流量:100%应变 | ISO 37 | 3.20 Mpa | |
流量:100%应变 | ASTM D412 | 3.40 Mpa |
aging | Test Condition | Test Method | TEKNOR APEX BELGIUM/4775B42 |
---|---|---|---|
Change rate of tensile strength in air | 100%应变,150°C,168hr,横向 | ASTM D573 | 2.0 % |
Change rate of ultimate elongation in air | 135°C,1000hr,横向 | ASTM D573 | -28 % |
Change rate of hardness (Shore) in the air | 邵氏A,150°C,168hr | ASTM D573 | 1.0 |
Change rate of tensile strength in air | 100%应变150°C,168hr,横向 | ISO 188 | 2.0 % |
Tensile stress change rate | 135°C,1000hr,断裂 | ISO 188 | -28 % |
volume change | 125°C,70hr,在IRM903油中 | ASTM D471 | 73 % |
Change rate of tensile strength in air | 100%应变135°C,1000hr,横向 | ISO 188 | 3.0 % |
135°C,1000hr,横向 | ISO 188 | -18 % | |
volume change | 125°C,70hr,在IRM903油中 | ISO 1817 | 73 % |
Tensile stress change rate | 150°C,168hr,断裂 | ISO 188 | -24 % |
Change rate of ultimate elongation in air | 150°C,168hr,横向 | ASTM D573 | -24 % |
Change rate of tensile strength in air | 100%应变,135°C,1000hr,横向 | ASTM D573 | 3.0 % |
Change rate of hardness (Shore) in the air | 邵氏A,135°C,1000hr | ISO 188 | -2.0 |
邵氏A,150°C,168hr | ISO 188 | 1.0 | |
Change rate of tensile strength in air | 135°C,1000hr,横向 | ASTM D573 | -18 % |
150°C,168hr,横向 | ASTM D573 | -19 % | |
Change rate of hardness (Shore) in the air | 邵氏A,135°C,1000hr | ASTM D573 | -2.0 |
Change rate of tensile strength in air | 150°C,168hr,横向 | ISO 188 | -19 % |
Contact Us
Get App
Top