Material Comparison
Product Info
Product Name
Brand Name
Usages
Properties
Certificates

PEI 2300R-7301 SABIC INNOVATIVE US
ULTEM™
Automotive Applications,Fitness equipment
Glass fiber reinforced,Flame retardant,enhance
--
--
--
--
--
--
--
--
--
--
--
--
--
--
--
Plastic Datasheets
| hardness | Test Condition | Test Method | SABIC INNOVATIVE US/2300R-7301 |
|---|---|---|---|
| Rockwell hardness | M-Scale | ASTM D785 | 114 |
| thermal performance | Test Condition | Test Method | SABIC INNOVATIVE US/2300R-7301 |
|---|---|---|---|
| Hot deformation temperature | 1.8MPa,Unannealed,6.40mm | ASTM D648 | 210 °C |
| 0.45MPa,Unannealed,6.40mm | ASTM D648 | 212 °C | |
| Linear coefficient of thermal expansion | MD:-20to150°C | ASTME831 | 2E-05 cm/cm/°C |
| RTI Elec | UL 746 | 180 °C | |
| RTI Imp | UL 746 | 170 °C | |
| RTI Str | UL 746 | 180 °C | |
| Vicat softening temperature | ASTM D15255 | 228 °C |
| mechanical properties | Test Condition | Test Method | SABIC INNOVATIVE US/2300R-7301 |
|---|---|---|---|
| Bending modulus | 100mmSpan | ASTM D790 | 8960 Mpa |
| bending strength | Break,100mmSpan | ASTM D790 | 228 Mpa |
| elongation | Break | ASTM D638 | 3.0 % |
| Tensile modulus | ASTM D638 | 9310 Mpa | |
| tensile strength | Yield | ASTM D638 | 169 Mpa |
| Break | ASTM D638 | 159 Mpa |
| Electrical performance | Test Condition | Test Method | SABIC INNOVATIVE US/2300R-7301 |
|---|---|---|---|
| Arc resistance | ASTM D495 | PLC6 | |
| Compared to the anti leakage trace index | CTI | UL 746 | PLC 4 |
| Dielectric constant | 1kHz | ASTM D150 | 3.70 |
| Dielectric strength | 1.60mm,inAir | ASTM D149 | 25 KV/mm |
| 1.60mm,in Oil | ASTM D149 | 30 KV/mm | |
| Dissipation factor | 1kHz | ASTM D150 | 1.5E-03 |
| 2.45GHz | ASTM D150 | 5.3E-03 | |
| High arc combustion index | HAI | UL 746 | PLC 4 |
| High voltage arc tracing rate | HVTR | UL 746 | PLC 3 |
| Hot wire ignition | HWI | UL 746 | PLC 1 |
| Volume resistivity | ASTM D257 | 3E+16 ohms·cm |
| Physical properties | Test Condition | Test Method | SABIC INNOVATIVE US/2300R-7301 |
|---|---|---|---|
| melt mass-flow rate | 337°C/6.6kg | ASTM D1238 | 5.3 g/10min |
| Shrinkage rate | MD:3.20mm | Internal Method | 0.20-0.40 % |
| Water absorption rate | 24hr | ASTM D570 | 0.16 % |
| Equilibrium,23°C | ASTM D570 | 0.90 % |
| impact performance | Test Condition | Test Method | SABIC INNOVATIVE US/2300R-7301 |
|---|---|---|---|
| Impact strength of cantilever beam gap | 3.20mm | ASTM D256 | 490 J/m |
| flammability | Test Condition | Test Method | SABIC INNOVATIVE US/2300R-7301 |
|---|---|---|---|
| Extreme Oxygen Index | ASTM D2863 | 50 % | |
| NBSSmokeDensity-Flaming,Ds,4min | ASTME662 | 1.60 | |
| UL flame retardant rating | 0.25mm | UL 94 | V-0 |
| 1.2mm | UL 94 | 5VA |