Material Comparison
Product Info
Product Name
Brand Name
Usages
Properties
Certificates

TPV 8191-55B100 CELANESE USA
Santoprene™
--
damping,Recyclable materials,Good forming performance,Ozone resistance,Chemical resistance,Oil resistant
--
--
--
--
--
--
--
--
--
--
--
--
--
--
--
Plastic Datasheets
| hardness | Test Condition | Test Method | CELANESE USA/8191-55B100 |
|---|---|---|---|
| Shore hardness | ShoreA,15Sec,23°C | ISO 868 | 53 |
| flammability | Test Condition | Test Method | CELANESE USA/8191-55B100 |
|---|---|---|---|
| UL flame retardant rating | 3.0mm | UL 94 | HB |
| 1.1mm | UL 94 | HB |
| elastomer | Test Condition | Test Method | CELANESE USA/8191-55B100 |
|---|---|---|---|
| elongation | Break,23°C,Across Flow | ISO 37 | 600 % |
| Break,23°C,Across Flow | ASTM D412 | 600 % | |
| Permanent compression deformation | 125°C,70hr | ISO 815 | 55 % |
| 125°C,70hr | ASTM D395B | 55 % |
| aging | Test Condition | Test Method | CELANESE USA/8191-55B100 |
|---|---|---|---|
| Change rate of hardness (Shore) in the air | ShoreA,23°C,168hr,inHydrochloricAcid,10% | ASTM D471 | 4.0 |
| ShoreA,125°C,168hr | ISO 188 | 8.0 | |
| ShoreA,23°C,168hr,inWater | ASTM D471 | 5.0 | |
| ShoreA,100°C,168hr | ASTM D573 | -4.0 | |
| ShoreA,100°C,168hr | ISO 188 | -4.0 | |
| ShoreA,23°C,168hr,inIRM903Oil | ASTM D471 | -33 | |
| ShoreA,125°C,168hr | ASTM D573 | 8.0 | |
| ShoreA,23°C,168hr,inSodiumHydroxide,50% | ASTM D471 | 4.0 | |
| ShoreA,23°C,168hr,inEthanol,95% | ASTM D471 | 2.0 | |
| Change rate of tensile strength in air | 125°C,168hr | ISO 188 | -61 % |
| 23°C,168hr,inHydrochloricAcid,10% | ISO 1817 | -1.0 % | |
| 23°C,168hr,在水中 | ISO 1817 | 2.0 % | |
| 100°C,168hr | ASTM D573 | -28 % | |
| 23°C,168hr,inSodiumHydroxide,50% | ISO 1817 | 1.0 % | |
| 23°C,168hr,inIRM903Oil | ISO 1817 | -85 % | |
| 100°C,168hr | ISO 188 | -28 % | |
| 23°C,168hr,inSodiumHydroxide,50% | ASTM D471 | 1.0 % | |
| 23°C,168hr,inIRM903Oil | ASTM D471 | -85 % | |
| 125°C,168hr | ASTM D573 | -61 % | |
| 23°C,168hr,inEthanol,95% | ASTM D471 | -17 % | |
| 23°C,168hr,在水中 | ASTM D471 | 2.0 % | |
| 23°C,168hr,inHydrochloricAcid,10% | ASTM D471 | -1.0 % | |
| 23°C,168hr,inEthanol,95% | ISO 1817 | -17 % | |
| Change rate of ultimate elongation in air | 23°C,168hr,inEthanol,95% | ASTM D471 | -3.0 % |
| 23°C,168hr,inIRM903Oil | ASTM D471 | -68 % | |
| 23°C,168hr,inSodiumHydroxide,50% | ASTM D471 | -7.0 % | |
| 23°C,168hr,在水中 | ASTM D471 | -12 % | |
| 125°C,168hr | ASTM D573 | -70 % | |
| 100°C,168hr | ASTM D573 | -14 % | |
| 23°C,168hr,inHydrochloricAcid,10% | ASTM D471 | -9.0 % | |
| Shore hardness | ShoreA,23°C,168hr,inSodiumHydroxide,50% | ISO 1817 | 4.0 |
| ShoreA,23°C,168hr,inHydrochloricAcid,10% | ISO 1817 | 4.0 | |
| ShoreA,23°C,168hr,inIRM903Oil | ISO 1817 | -33 | |
| ShoreA,23°C,168hr,inEthanol,95% | ISO 1817 | 2.0 | |
| ShoreA,23°C,168hr,inWater | ISO 1817 | 5.0 | |
| Tensile stress change rate | 23°C,168hr,inIRM903Oil,Break | ISO 1817 | -68 % |
| 23°C,168hr,inEthanol,95%,Break | ISO 1817 | -3.0 % | |
| 23°C,168hr,在水中,Break | ISO 1817 | -12 % | |
| 125°C,168hr,Break | ISO 188 | -70 % | |
| 23°C,168hr,inSodiumHydroxide,50%,Break | ISO 1817 | -7.0 % | |
| 23°C,168hr,inHydrochloricAcid,10%,Break | ISO 1817 | -9.0 % | |
| 100°C,168hr,Break | ISO 188 | -14 % |