Material Comparison
Product Info
Product Name
Brand Name
Usages
Properties
Certificates

TPU 95AU(H)T COVESTRO SHANGHAI
Texin®
Cable sheath,Engineering accessories,pipeline,Profile,Hydraulic applications
Hydrolysis resistance,Low temperature flexibili
--
--
--
--
--
--
--
--
--
--
--
--
--
--
--
Plastic Datasheets
hardness | Test Condition | Test Method | COVESTRO SHANGHAI/95AU(H)T |
---|---|---|---|
Shore hardness | Shore A | ASTM D2240 | 95 |
thermal performance | Test Condition | Test Method | COVESTRO SHANGHAI/95AU(H)T |
---|---|---|---|
Brittle temperature | ASTM D746 | -53.9 °C |
mechanical properties | Test Condition | Test Method | COVESTRO SHANGHAI/95AU(H)T |
---|---|---|---|
elongation | Break | ASTM D638 | 500 % |
tensile strength | Yield | ASTM D638 | 6.55 Mpa |
Physical properties | Test Condition | Test Method | COVESTRO SHANGHAI/95AU(H)T |
---|---|---|---|
Shrinkage rate | 3.20 mm,Flow | ASTM D955 | 1.1 - 1.4 % |
flammability | Test Condition | Test Method | COVESTRO SHANGHAI/95AU(H)T |
---|---|---|---|
UL flame retardant rating | 1.0 mm | UL 94 | HB |
injection | Test Condition | Test Method | COVESTRO SHANGHAI/95AU(H)T |
---|---|---|---|
Back pressure | 0.172 to 0.689 Mpa | ||
drying temperature | 82 °C | ||
drying time | 3.0 hr | ||
Exhaust hole depth | 0.013 to 0.038 mm | ||
Mold temperature | 32 to 71 °C | ||
Processing (melt) temperature | 193 to 204 °C | ||
Screw speed | 25 to 75 rpm | ||
Spray nozzle temperature | 182 to 204 °C | ||
Suggested maximum moisture content | 0.080 % | ||
Temperature at the front of the material cylinder | 182 to 204 °C | ||
Temperature at the rear of the barrel | 160 to 182 °C | ||
Temperature in the middle of the barrel | 171 to 193 °C |