Material Comparison
Product Info
Product Name
Brand Name
Usages
Properties
Certificates

TPEE G3548L DUPONT LUXEMBOURG
BEXLOY®
Automotive Applications、Electrical applications
UV resistance、Thermal stability
--
--
--
--
--
--
--
--
--
--
--
--
--
--
--
Plastic Datasheets
Other performance | Test Condition | Test Method | DUPONT LUXEMBOURG/G3548L |
---|---|---|---|
Wear resistant and flexible incision growth performance | ASTM D-1052 | >1×10 |
Basic performance | Test Condition | Test Method | DUPONT LUXEMBOURG/G3548L |
---|---|---|---|
24-hour water absorption rate | ASTM D-570 | 5 % |
Mechanical properties | Test Condition | Test Method | DUPONT LUXEMBOURG/G3548L |
---|---|---|---|
Tensile | 5%伸长 | ASTM D-638 | 1.7 Mpa |
durometer hardness | ASTM D-2240 | 35 | |
Ezo impact strength | 23℃ | ASTM D-256 | 不破裂 J/m |
Rubbing modulus | 23℃ | ASTM D-790 | 32.4 Mpa |
Tensile | 10%伸长 | ASTM D-638 | 2.6 Mpa |
Fracture tensile force | ASTM D-638 | 10.3 Mpa | |
ELONGATION AT BREAK | ASTM D-638 | 200 % | |
Initial tear resistance performance | ASTM D-1004 | 51 kN/m |
physical property | Test Condition | Test Method | DUPONT LUXEMBOURG/G3548L |
---|---|---|---|
melt mass-flow rate | ASTM D-1238 | 10 g/10min | |
Taber wear amount | H 18轮 | ASTM D-1044 | 310 mg/1000rev |
CS-17轮 | ASTM D-1044 | 30 mg/1000rev |
Thermal performance | Test Condition | Test Method | DUPONT LUXEMBOURG/G3548L |
---|---|---|---|
heat distortion temperature | @0.5Mpa | ASTM D-648 | N/A °C |
vicat | ASTM D-1525 | 77 °C | |
heat distortion temperature | @0.18Mpa | ASTM D-648 | N/A °C |
melting point | ASTM D-3418 | 156 °C |