Material Comparison
Product Info
Product Name
Brand Name
Usages
Properties
Certificates

TPU GP65AE NAT 030 Luborun
--
Aerospace Applications
aromatic
--
--
--
--
--
--
--
--
--
--
--
--
--
--
--
Plastic Datasheets
Mechanical properties | Test Condition | Test Method | Luborun/GP65AE NAT 030 |
---|---|---|---|
tensile strength | 断裂 | ISO 527-3 | 28.0 MPa |
tear strength | -- 2 | ISO 34-1 | 73 kN/m |
Resilience | ISO 4662 | 56 % | |
wear resistance | Injection molded | ISO 4649 | 34.0 mm³ |
compression set | 22°C, 70.0 hr | ISO 815 | 16 % |
tensile strength | 50%应变 | ISO 527-3 | 1.50 MPa |
elongation | 断裂 | ISO 527-3 | 1000 % |
Tensile modulus | 注塑 | ISO 527-2 | 3.00 MPa |
physical property | Test Condition | Test Method | Luborun/GP65AE NAT 030 |
---|---|---|---|
density | ISO 2781 | 1.18 g/cm³ | |
Shore hardness | 支撐 A | ISO 868 | 63 |
melt mass-flow rate | 170°C/8.7 kg | 10 to 25 g/10 min |
Thermal performance | Test Condition | Test Method | Luborun/GP65AE NAT 030 |
---|---|---|---|
vicat | ISO 306/A50 | 74.0 ℃ |
Contact Us
Get App
Top