ASA Generic ASA+PC Generic
--
--
--
--
--
--
--
--
--
--
--
--
--
--
--
--
--
--

Plastic Datasheets

hardnessTest ConditionTest MethodGeneric/Generic ASA+PC
Ball Pressure TestISO 2039-188.7to110 MPa
Rockwell hardness23°CASTM D785109to116
thermal performanceTest ConditionTest MethodGeneric/Generic ASA+PC
Hot deformation temperature1.8MPa,UnannealedASTM D64887.7to113 °C
0.45MPa,UnannealedISO 75-2/B98.4to132 °C
1.8MPa,UnannealedISO 75-2/A87.2to122 °C
0.45MPa,UnannealedASTM D648102to130 °C
Linear coefficient of thermal expansionMDASTME8317.2E-5到7.3E-5 cm/cm/°C
TDISO 11359-27.1E-5到7.8E-5 cm/cm/°C
MDISO 11359-21.0E-5到8.6E-5 cm/cm/°C
TDASTME8317.2E-5到7.9E-5 cm/cm/°C
Vicat softening temperature--ISO 306102to139 °C
--ASTM D1525104to138 °C
mechanical propertiesTest ConditionTest MethodGeneric/Generic ASA+PC
Bending modulus23°CISO 1782000to2640 MPa
23°CASTM D7902080to2770 MPa
bending strengthYield,23°CASTM D79081.7to95.4 MPa
23°CASTM D79068.0to94.0 MPa
23°CISO 17872.8to97.5 MPa
elongationBreak,23°CISO 527-236to80 %
Yield,23°CASTM D6383.7to6.1 %
Yield,23°CISO 527-22.3to8.7 %
Break,23°CASTM D63823to100 %
Tensile modulus23°CASTM D6382540to2720 MPa
23°CISO 527-22120to2760 MPa
tensile strengthBreak,23°CASTM D63844.0to66.0 MPa
Yield,23°CISO 527-254.6to62.4 MPa
Break,23°CISO 527-239.0to64.3 MPa
Yield,23°CASTM D63852.9to65.6 MPa
Electrical performanceTest ConditionTest MethodGeneric/Generic ASA+PC
Surface resistivityIEC 600931.0E+13到1.0E+15 ohms
Volume resistivity23°CIEC 600931.0E+13到1.0E+15 ohms·cm
Physical propertiesTest ConditionTest MethodGeneric/Generic ASA+PC
density23°CISO 11831.11to1.20 g/cm³
--ASTM D7921.10to1.25 g/cm³
melt mass-flow rate260°C/5.0kgISO 113319to40 g/10min
260°C/5.0kgASTM D123814to45 g/10min
Melt Volume Flow Rate (MVR)260°C/5.0kgISO 113317.0to26.0 cm³/10min
Shrinkage rateMD:23°CASTM D9550.50to0.60 %
23°CISO 294-40.59to0.70 %
Water absorption rateEquilibrium,23°C,50%RHISO 620.20to0.30 %
23°C,24hrASTM D5700.10to0.25 %
Saturation,23°CISO 620.60to1.0 %
impact performanceTest ConditionTest MethodGeneric/Generic ASA+PC
Charpy Notched Impact Strength23°CISO 1795.0to62 kJ/m²
Dart impact23°CASTM D376335.3to47.9 J
Impact strength of cantilever beam gap23°CISO 18016to61 kJ/m²
23°CASTM D256140to600 J/m
flammabilityTest ConditionTest MethodGeneric/Generic ASA+PC
Hot filament ignition temperatureIEC 60695-2-13550to960 °C