Material Comparison
Product Info
Product Name
Brand Name
Usages
Properties
Certificates

ULDPE 4404G STYRON US
ATTANE™
chip,film,Mainly used for packaging
optical performance ,High toughness,High toughness and optica,Certified by Canadian HPF
--
--
--
--
--
--
--
--
--
--
--
--
--
--
--
Plastic Datasheets
Basic Performance | Test Condition | Test Method | STYRON US/4404G |
---|---|---|---|
density | ASTM D792 | 0.904 g/cm³ | |
melt mass-flow rate | ASTM D1238 | 4 g/10min |
thermal performance | Test Condition | Test Method | STYRON US/4404G |
---|---|---|---|
Melting temperature | Internal Method | 124 °C | |
Vicat softening temperature | ASTM D-1525 | 71 °C | |
ASTM D1525 | 71.1 °C |
film | Test Condition | Test Method | STYRON US/4404G |
---|---|---|---|
Carbon dioxide transmittance | 23°C,50.8μm | Internal Method | 2000 cm³·mm/m²/atm/24hr |
Dart impact | 20μm | ASTM D1709B | >850 g |
51μm | ASTM D1709B | >850 g | |
Elmendorf tear strength | MD:20μm | ASTM D1922 | 330 g |
TD:20μm | ASTM D1922 | 500 g | |
MD:51μm | ASTM D1922 | 960 g | |
TD:51μm | ASTM D1922 | 1100 g | |
elongation | MD:Break,51μm | ASTM D882 | 660 % |
TD:Break,51μm | ASTM D882 | 710 % | |
MD:Break,20μm | ASTM D882 | 500 % | |
TD:Break,20μm | ASTM D882 | 710 % | |
Oxygen permeability | 23°C,51μm | ASTM D3985 | 450 cm³·mm/m²/atm/24hr |
Secant modulus | 2%Secant,TD:51μm | ASTM D882 | 63.0 Mpa |
2%Secant,MD:20μm | ASTM D882 | 58.8 Mpa | |
2%Secant,TD:20μm | ASTM D882 | 64.7 Mpa | |
2%Secant,MD:51μm | ASTM D882 | 62.6 Mpa | |
tensile strength | TD:Break,20μm | ASTM D882 | 29.1 Mpa |
MD:Break,20μm | ASTM D882 | 36.9 Mpa | |
MD:Yield,20μm | ASTM D882 | 7.00 Mpa | |
TD:Yield,51μm | ASTM D882 | 6.34 Mpa | |
TD:Break,51μm | ASTM D882 | 32.4 Mpa | |
MD:Break,51μm | ASTM D882 | 32.6 Mpa | |
MD:Yield,51μm | ASTM D882 | 6.76 Mpa | |
TD:Yield,20μm | ASTM D882 | 4.92 Mpa | |
Thin film puncture strength | 51μm | Internal Method | 17.5 J/cm³ |
20μm | Internal Method | 18.9 J/cm³ | |
Water vapor permeability | 51μm | ASTMF1249 | 0.85 g·mm/m²/atm/24hr |
mechanical properties | Test Condition | Test Method | STYRON US/4404G |
---|---|---|---|
Elongation at Break | MD | ASTM D-882 | 664 % |
TD | ASTM D-882 | 714 % | |
Puncture intensity | 陶氏企业测试 | 17 J/cm³ | |
Tensile modulus | MD,3% Secant | ASTM D-882 | 63 Mpa |
TD,2% Secant | ASTM D-882 | 63 Mpa | |
tensile strength | TD,Break | ASTM D-882 | 32 Mpa |
MD,Break | ASTM D-882 | 33 Mpa | |
Yield,TD | ASTM D-882 | 5 Mpa | |
Yield,MD | ASTM D-882 | 7 Mpa |
Physical properties | Test Condition | Test Method | STYRON US/4404G |
---|---|---|---|
melt mass-flow rate | 190°C/2.16kg | ASTM D1238 | 4.0 g/10min |
optical performance | Test Condition | Test Method | STYRON US/4404G |
---|---|---|---|
gloss | 45°,20.3μm | ASTM D2457 | 92 |
45°,50.8μm | ASTM D2457 | 90 | |
45° | ASTM D-2457 | 90 | |
transparency | 50.8μm | ASTM D1746 | 99.0 |
ASTM D-1746 | 99 | ||
20.3μm | ASTM D1746 | 99.0 | |
turbidity | ASTM D-1003 | 1.8 % | |
20.3μm | ASTM D1003 | 0.60 % | |
50.8μm | ASTM D1003 | 1.8 % |