PPS A310M-X11 TORAY JAPAN
Torelina®
--
--
--
--
--
--
--
--
--
--
--
--
--
--
--
--
--
Plastic Datasheets
| Basic Performance | Test Condition | Test Method | TORAY JAPAN/A310M-X11 |
|---|---|---|---|
| Water absorption rate | ASTM D-570 | 0.02 % |
| thermal performance | Test Condition | Test Method | TORAY JAPAN/A310M-X11 |
|---|---|---|---|
| Combustibility | UL -94 | V-0 | |
| Hot deformation temperature | 1.82MPa | ASTM D-648 | >260 °C |
| Linear coefficient of thermal expansion | 垂重方向 | ASTM D-696 | 2.4 |
| Flow | ASTM D-696 | 1.6 | |
| Melting temperature | DSC | 278 °C |
| mechanical properties | Test Condition | Test Method | TORAY JAPAN/A310M-X11 |
|---|---|---|---|
| abrasion | ASTM D-1044 | 70 mg/1000回 | |
| bending strength | ASTM D-790 | 200 Mpa | |
| ASTM D-790 | 17.6 GPa | ||
| Elongation at Break | ASTM D-732 | 60 | |
| Friction coefficient | 对钢 | ASTM D-1894 | 0.30 |
| Impact strength of cantilever beam gap | Unnotched23℃ | ASTM D-256 | 20 KJ/m |
| Notched23℃ | ASTM D-256 | 90 J/m | |
| limiting pv value | 东丽法 | 815 KJ/m | |
| Shore hardness | ASTM D-785 | 123 洛氏 | |
| tensile strength | ASTM D-638 | 140 Mpa | |
| ASTM D-638 | 1.2 % |
| Electrical performance | Test Condition | Test Method | TORAY JAPAN/A310M-X11 |
|---|---|---|---|
| Arc resistance | W电极 | ASTM D-495 | 182 秒 |
| Dielectric constant | 10 | ASTM D-150 | 5.8 |
| Dielectric strength | ASTM D-149 | 15 MV/m | |
| Induced positive connection | 10 | ASTM D-150 | 0.002 |
| Inherent resistance of volume | ASTM D-257 | 10 Ω.m |
| Physical properties | Test Condition | Test Method | TORAY JAPAN/A310M-X11 |
|---|---|---|---|
| 320℃,98MPa,1mm厚,Flow长 | 东丽法 | 90 | |
| Shrinkage rate | Flow | 东丽法 | 0.15 % |
| 垂重方向 | 东丽法 | 0.55 % |