| mechanical properties | Test Condition | Test Method | SABIC INNOVATIVE US/OL-4030 |
|---|---|---|---|
| elongation | Break | ASTM D638 | 0.60 % |
| bending strength | ISO 178 | 56.0 Mpa | |
| Break,50.0mmSpan | ASTM D790 | 65.0 Mpa | |
| tensile strength | Break | ASTM D638 | 21.0 Mpa |
| Tensile strain | Break | ISO 527-2/5 | 0.60 % |
| Bending modulus | ISO 178 | 3320 Mpa | |
| 50.0mmSpan | ASTM D790 | 3870 Mpa | |
| Tensile modulus | ISO 527-2/1 | 3370 Mpa | |
| ASTM D638 | 3590 Mpa | ||
| tensile strength | Break | ISO 527-2/5 | 20.0 Mpa |
| thermal performance | Test Condition | Test Method | SABIC INNOVATIVE US/OL-4030 |
| Hot deformation temperature | 1.8MPa,Unannealed,3.20mm | ASTM D648 | 108 °C |
| 1.8MPa,Unannealed,64.0mmSpan | ISO 75-2/Af | 109 °C | |
| Linear coefficient of thermal expansion | MD:-30to30°C | ASTM D696 | 6E-05 cm/cm/°C |
| TD:-30to30°C | ASTM D696 | 6.6E-05 cm/cm/°C | |
| Hot deformation temperature | 0.45MPa,Unannealed,3.20mm | ASTM D648 | 175 °C |
| 0.45MPa,Unannealed,64.0mmSpan | ISO 75-2/Bf | 178 °C | |
| Physical properties | Test Condition | Test Method | SABIC INNOVATIVE US/OL-4030 |
| Shrinkage rate | MD:24hr | ASTM D955 | 0.90-2.0 % |
| Water absorption rate | Equilibrium,23°C,50%RH | ISO 62 | 0.040 % |
| Shrinkage rate | TD:24hr | ASTM D955 | 1.0-3.0 % |
| Water absorption rate | 24hr,50%RH | ASTM D570 | 0.020 % |
| impact performance | Test Condition | Test Method | SABIC INNOVATIVE US/OL-4030 |
| Dart impact | 23°C,TotalEnergy | ASTM D3763 | 1.00 J |
| Impact strength of cantilever beam gap | 23°C | ISO 180/1A | 2.2 kJ/m² |
| Multi axis Instrumented Impact Energy | ISO 6603-2 | 0.400 J | |
| Suspended wall beam without notch impact strength | 23°C | ISO 180/1U | 4.8 kJ/m² |