PC DF-1006 BK82025 SABIC INNOVATIVE US
LNP™ THERMOCOMP™
Plastic bag、Medical and nursing suppl
Low extract、Easy to form、Easy to demould
--
--
--
--
--
--
--
--
--
--
--
--
--
--
--
Plastic Datasheets
Thermal Properties | Test Condition | Test Method | SABIC INNOVATIVE US/DF-1006 BK82025 |
---|---|---|---|
Deflection Temperature Under Load? | 0.45 MPa, 未退火, 4.00 mm, 64.0 mm 跨距 6 | ISO 75-2/Bf | 146 °C |
1.8 MPa, 未退火, 4.00 mm, 64.0 mm 跨距 6 | ISO 75-2/Af | 142 °C | |
1.8 MPa, 未退火, 3.20 mm | ASTM D648 | 140 °C | |
0.45 MPa, 未退火, 3.20 mm | ASTM D648 | 144 °C |
Injection | Test Condition | Test Method | SABIC INNOVATIVE US/DF-1006 BK82025 |
---|---|---|---|
Suggested Max Moisture | 0.020 % | ||
Middle Temperature | 310 到 320 °C | ||
Processing (Melt) Temp | 305 到 325 °C | ||
Drying Time | 4.0 hr | ||
Rear Temperature | 295 到 305 °C | ||
Drying Temperature | 120 °C | ||
Front Temperature | 320 到 330 °C | ||
Back Pressure | 0.200 到 0.300 Mpa | ||
Mold Temperature | 80 到 110 °C | ||
Screw Speed | 30 到 60 rpm |
Physical | Test Condition | Test Method | SABIC INNOVATIVE US/DF-1006 BK82025 |
---|---|---|---|
Moisture Absorption | 24 hr, 50% RH | ASTM D570 | 0.070 % |
平衡, 23°C, 50% RH | ISO 62 | 0.070 % |
Mechanical Properties | Test Condition | Test Method | SABIC INNOVATIVE US/DF-1006 BK82025 |
---|---|---|---|
Tensile Elongation | 断裂 3 | ASTM D638 | 3.2 % |
断裂 | ISO 527-2/5 | 7.5 % | |
Flexural Strength | 断裂, 50.0 mm 跨距 | ASTM D790 | 149 Mpa |
Tensile Modulus | ASTM D638 | 8630 Mpa | |
Tensile Strength | 断裂 | ISO 527-2/5 | 114 Mpa |
Tensile Elongation | 屈服 3 | ASTM D638 | 2.7 % |
Flexural Modulus | -- 5 | ISO 178 | 7860 Mpa |
50.0 mm 跨距 4 | ASTM D790 | 8230 Mpa | |
Tensile Strength | 断裂 3 | ASTM D638 | 114 Mpa |
Impact Properties | Test Condition | Test Method | SABIC INNOVATIVE US/DF-1006 BK82025 |
---|---|---|---|
Unnotched Izod Impact Strength | 23°C | ASTM D4812 | 910 J/m |
23°C 6 | ISO 180/1U | 58 kJ/m² |