Material Comparison
Product Info
Product Name
Brand Name
Usages
Properties
Certificates

PA6 Quadrant EPP Nylatron® GSM Blue Mitsubishi Chemical Advanced Materials
--
--
--
--
--
--
--
--
--
--
--
--
--
--
--
--
--
--
Plastic Datasheets
Impact resistance | Test Condition | Test Method | Mitsubishi Chemical Advanced Materials/Quadrant EPP Nylatron® GSM Blue |
---|---|---|---|
Impact strength of cantilever beam gap | ASTM D256A | 48 J/m |
hardness | Test Condition | Test Method | Mitsubishi Chemical Advanced Materials/Quadrant EPP Nylatron® GSM Blue |
---|---|---|---|
Rockwell hardness | M级 | ASTM D785 | 80 |
R级 | ASTM D785 | 117 |
Supplementary Information | Test Condition | Test Method | Mitsubishi Chemical Advanced Materials/Quadrant EPP Nylatron® GSM Blue |
---|---|---|---|
limiting pv value | 内部方法 | 0.193 MPa·m/s |
Electrical performance | Test Condition | Test Method | Mitsubishi Chemical Advanced Materials/Quadrant EPP Nylatron® GSM Blue |
---|---|---|---|
Surface Resistivity | 内部方法 | >1.0E+13 ohms |
Mechanical properties | Test Condition | Test Method | Mitsubishi Chemical Advanced Materials/Quadrant EPP Nylatron® GSM Blue |
---|---|---|---|
tensile strength | 极限 | ASTM D638 | 68.9 MPa |
elongation | 断裂 | ASTM D638 | 30 % |
bending strength | 屈服 | ASTM D790 | 103 MPa |
compressive strength | 10%应变 | ASTM D695 | 89.6 MPa |
Tensile modulus | ASTM D638 | 3450 MPa | |
Flexural modulus | ASTM D790 | 3450 MPa | |
Compression Modulus | ASTM D695 | 2930 MPa | |
Wear factor | ASTM D3702 | 130 10^-8mm³/N·m | |
coefficient of friction | 与钢-静态 | 内部方法 | 0.18 |
flammability | Test Condition | Test Method | Mitsubishi Chemical Advanced Materials/Quadrant EPP Nylatron® GSM Blue |
---|---|---|---|
UL flame retardant rating | 3.2mm | UL 94 | HB |
physical property | Test Condition | Test Method | Mitsubishi Chemical Advanced Materials/Quadrant EPP Nylatron® GSM Blue |
---|---|---|---|
Water absorption rate | 饱和 | ASTM D570 | 6.0 % |
24hr | ASTM D570 | 0.30 % | |
density | ASTM D792 | 1.15 g/cm³ |
Thermal performance | Test Condition | Test Method | Mitsubishi Chemical Advanced Materials/Quadrant EPP Nylatron® GSM Blue |
---|---|---|---|
Heat distortion temperature | 1.8MPa,未退火,HDT | ASTM D648 | 93.3 °C |
Crystallization peak temperature | DSC | ASTM D3418 | 216 °C |
Linear coefficient of thermal expansion | MD2:-40到149°C | ASTME831 | 9.9E-05 cm/cm/°C |
Maximum operating temperature LongTerm, Air | 93 °C |
Contact Us
Get App
Top