Material Comparison
Product Info
Product Name
Brand Name
Usages
Properties
Certificates

LCP A950 JAPAN POLYPLASTIC
LAPEROS®
Automotive sector,Camera applications,Electrical field,Electronic field,Optical applications
Corrosion resistance,Thermal stability,Weather resistance,High rigidity,high strength,damping,Flame retardant
UL
--
--
--
--
--
--
--
--
--
--
--
--
--
--
--
Plastic Datasheets
| Basic Performance | Test Condition | Test Method | JAPAN POLYPLASTIC/A950 |
|---|---|---|---|
| density | ISO 1183 | 1400 kg/m | |
| Water absorption rate | 23℃/50rh | ISO 62 | 0.030 % |
| thermal performance | Test Condition | Test Method | JAPAN POLYPLASTIC/A950 |
|---|---|---|---|
| Combustibility | UL 94 | V-0 | |
| Hot deformation temperature | 1.80MPa | ISO 75-1 | 187 °C |
| Linear coefficient of thermal expansion | normal | ISO 11359-1 | 0.000038 cm/cm℃ |
| parallel | ISO 11359-1 | 4E-06 cm/cm℃ | |
| Vicat softening temperature | 50℃/h 50N | ISO 306 | 145 °C |
| mechanical properties | Test Condition | Test Method | JAPAN POLYPLASTIC/A950 |
|---|---|---|---|
| Bending modulus | 23℃ | ISO 178 | 9100 Mpa |
| bending strength | 23℃ | ISO 178 | 158 Mpa |
| Charpy Notched Impact Strength | 23℃ | ISO 179/1eA | 95.0 KJ/m |
| -30℃ | ISO 179/1eU | 53.0 KJ/m | |
| 23℃ | ISO 179/1eU | 267 KJ/m | |
| Fracture strain | ISO 527-1 | 3.4 % | |
| Fracture stress | ISO 527-1 | 182 Mpa | |
| Impact strength of cantilever beam gap | 23℃ | ISO 180/1A | 95.0 KJ/m |
| Suspended wall beam without notch impact strength | 23℃ | ISO 180/1U | 252 KJ/m |
| Tensile creep modulus | 1hr | ISO 899-1 | 9000 Mpa |
| 1000hr | ISO 899-1 | 6600 Mpa | |
| Tensile modulus | ISO 527-1 | 10600 Mpa |
| Electrical performance | Test Condition | Test Method | JAPAN POLYPLASTIC/A950 |
|---|---|---|---|
| Dielectric loss | 100Hz | IEC 60250 | 0.016 |
| 1000Hz | IEC 60250 | 0.020 | |
| Dielectric strength | IEC 60243-1 | 47 KV/mm | |
| Relative permittivity | 100Hz | IEC 60250 | 3.20 |
| 1000Hz | IEC 60250 | 3.00 | |
| Surface resistivity | IEC 60093 | 1E+14 ohms | |
| Volume resistivity | IEC 60093 | 1E+13 ohm.m |
| Physical properties | Test Condition | Test Method | JAPAN POLYPLASTIC/A950 |
|---|---|---|---|
| Shrinkage rate | parallel | ISO 2577 | 0.70 % |
| normal | ISO 2577 | 0.0 % |