Material Comparison
Product Info
Product Name
Brand Name
Usages
Properties
Certificates

TPU DP9370A COVESTRO GERMANY
Desmopan®
Laptop case,Printer
Aging resistance,Wear resistance
--
--
--
--
--
--
--
--
--
--
--
--
--
--
--
Plastic Datasheets
| hardness | Test Condition | Test Method | COVESTRO GERMANY/DP9370A |
|---|---|---|---|
| Shore hardness | ShoreA,3Sec | ISO 8682 | 70 |
| mechanical properties | Test Condition | Test Method | COVESTRO GERMANY/DP9370A |
|---|---|---|---|
| TensileStorageModulus | 60°C | ISO 6721-1 | 9.00 Mpa |
| -20°C | ISO 6721-1 | 125 Mpa | |
| 20°C | ISO 6721-1 | 11.0 Mpa | |
| Tensile strain | Break,23°C | DIN 53504 | 740 % |
| tensile strength | 100%Strain,23°C | DIN 53504 | 3.50 Mpa |
| Break,23°C | DIN 53504 | 25.7 Mpa | |
| 10%Strain | DIN 53504 | 1.00 Mpa | |
| 300%Strain,23°C | DIN 53504 | 6.70 Mpa | |
| Wear resistance | 23°C | ISO 4649-A | 69.0 mm³ |
| impact performance | Test Condition | Test Method | COVESTRO GERMANY/DP9370A |
|---|---|---|---|
| ImpactResilience | 23°C | ISO 4662 | 63 % |
| elastomer | Test Condition | Test Method | COVESTRO GERMANY/DP9370A |
|---|---|---|---|
| Permanent compression deformation | 70°C,24hr | ISO 815 | 49 % |
| 23°C,72hr | ISO 815 | 22 % | |
| tear strength | 23°C | ISO 34-1 | 39 kN/m |