Technical Data Sheet Compareoptical performance Test Condition Test Method Test Result Refractive index ASTM D542 1.586 transmissivity 2540 μm ASTM D1003 88.0 % turbidity 2540 μm ASTM D1003 1.0 %
impact performance Test Condition Test Method Test Result Impact strength of cantilever beam gap ASTM D1822 546 kJ/m² Dart impact 23°C ASTM D3029 169 J Suspended wall beam without notch impact strength 23°C ASTM D4812 3200 J/m
flammability Test Condition Test Method Test Result UL flame retardant rating 0.76 mm UL 94 HB
mechanical properties Test Condition Test Method Test Result Taber abraser 1000 Cycles, 1000 g, CS-17 Wheel ASTM D1044 10.0 mg bending strength Yield, 50.0 mm Span ASTM D790 93.0 Mpa Bending modulus 50.0 mm Span ASTM D790 2340 Mpa elongation Break ASTM D638 110 % elongation Yield ASTM D638 7.0 % tensile strength Break ASTM D638 65.0 Mpa tensile strength Yield ASTM D638 62.0 Mpa
injection Test Condition Test Method Test Result Processing (melt) temperature 310 to 330 °C Mold temperature 80 to 115 °C Back pressure 0.300 to 0.700 Mpa Screw speed 40 to 70 rpm Exhaust hole depth 0.025 to 0.076 mm drying temperature 120 °C drying time 3.0 to 4.0 hr Suggested maximum moisture content 0.020 % Suggested injection volume 40 to 60 % Temperature at the rear of the barrel 290 to 310 °C Temperature in the middle of the barrel 300 to 320 °C Temperature at the front of the material cylinder 310 to 330 °C Spray nozzle temperature 305 to 325 °C
thermal performance Test Condition Test Method Test Result thermal conductivity ASTM C177 0.19 W/m/K RTI Elec UL 746 130 °C RTI Imp UL 746 130 °C specific heat ASTM C351 1250 J/kg/°C Linear coefficient of thermal expansion -40 to 95°C,Flow ASTM E831 6.8E-5 cm/cm/°C Vicat softening temperature ASTM D15255 154 °C Hot deformation temperature 1.8 MPa, Unannealed, 6.40 mm ASTM D648 132 °C Hot deformation temperature 0.45 MPa, Unannealed, 6.40 mm ASTM D648 137 °C RTI UL 746 130 °C
Physical properties Test Condition Test Method Test Result Outdoor applicability UL 746C f1 Water absorption rate Equilibrium, 100°C ASTM D570 0.58 % Water absorption rate Equilibrium, 23°C ASTM D570 0.35 % Water absorption rate 24 hr ASTM D570 0.15 % Shrinkage rate 3.20 mm,Flow Internal Method 0.50 - 0.70 % melt mass-flow rate 300°C/1.2 kg ASTM D1238 7.0 g/10 min Specific volume ASTM D792 0.830 cm³/g
Electrical performance Test Condition Test Method Test Result Volume resistivity ASTM D257 > 1.0E+17 ohms·cm Dielectric strength 3.20 mm, in Air ASTM D149 15 KV/mm Dielectric constant 60 Hz ASTM D150 3.17 Dielectric constant 50 kHz ASTM D150 3.17 Dielectric constant 1 MHz ASTM D150 2.96 Dissipation factor 50 Hz ASTM D150 9.0E-4 Dissipation factor 60 Hz ASTM D150 9.0E-4 Dissipation factor 1 MHz ASTM D150 0.010 Compared to the anti leakage trace index UL 746 PLC 2 High arc combustion index UL 746 PLC 1 High voltage arc tracing rate UL 746 PLC 2 Hot wire ignition UL 746 PLC 4
hardness Test Condition Test Method Test Result Rockwell hardness R-Scale ASTM D785 118 Rockwell hardness M-Scale ASTM D785 70
IMPORTANT NOTES: Plas.com collected the data in the data sheet from the material manufacturers. Plas.com makes the best effort to improve the accuracy of the data, but has no responsibility for the data. We strongly recommend verifying the validity of the data with the material manufacturers before making a final decision.