plas
ورود

ECTFE Halar® 700 HC SOLVAY BELGIUM

0

برگه داده فنی

flammabilityشرایط آزمونروش آزموننتیجه آزمون
Extreme Oxygen IndexASTM D2863>52 %
UL flame retardant ratingUL 94V-0
mechanical propertiesشرایط آزمونروش آزموننتیجه آزمون
Tensile modulus23°CASTM D8821320 MPa
tensile strengthYield,23°CISO 527-328.5 MPa
tensile strengthBreak,23°CISO 527-341.4 MPa
elongationYield,23°CISO 527-35.0 %
elongationBreak,23°CISO 527-3310 %
Friction coefficientItself - DynamicASTM D18940.20
Taber abraser1000Cycles,500g,CS-17WheelASTM D406016.5 mg
thermal performanceشرایط آزمونروش آزموننتیجه آزمون
Fusion temperatureASTM D341824.0 J/g
thermal stabilityTGA359 °C
Brittle temperatureASTM D746A<-50.0 °C
Glass transition temperatureDMA70.0 °C
Melting temperatureASTM D3418200 °C
Crystallization peak temperatureDSCASTM D3418180 °C
thermal conductivity23°CASTMC1770.18 W/m/K
Crystallization peak temperatureASTM D341822.7 J/g
Physical propertiesشرایط آزمونروش آزموننتیجه آزمون
densityASTM D7921.70 g/cm³
melt mass-flow rate275°C/2.16kgASTM D12387.0to10 g/10min
Water absorption rateEquilibriumASTM D570<0.10 %
Electrical performanceشرایط آزمونروش آزموننتیجه آزمون
Dielectric strength23°C,3.20mmASTM D14914 kV/mm
Dielectric constant23°C,1MHzASTM D1502.57
hardnessشرایط آزمونروش آزموننتیجه آزمون
Shore hardnessShoreDASTM D224074
filmشرایط آزمونروش آزموننتیجه آزمون
Tear strength of pants shape23°C,3.20mmDIN 53363420.0 kN/m
نکات مهم: Plas.com داده‌های برگه فنی را از تولیدکنندگان مواد جمع‌آوری کرده است. Plas.com تمام تلاش خود را برای افزایش دقت داده‌ها انجام می‌دهد، اما هیچ مسئولیتی در قبال داده‌ها ندارد. اکیداً توصیه می‌شود که صحت داده‌ها را با تولیدکنندگان مواد تأیید کنید پیش از آنکه تصمیم نهایی بگیرید.