physical property | شرایط آزمون | روش آزمون | نتیجه آزمون |
---|
Mooney viscosity | ML1+10,121°C3 | ASTM D1646 | 61 MU |
Fluorine content | | 内部方法 | 66 % |
solubility | | | 酮类和酯类 |
density | | ASTM D792 | 1.81 g/cm³ |
Mooney viscosity | ML1+10,121°C2 | ASTM D1646 | 31 MU |
hardness | شرایط آزمون | روش آزمون | نتیجه آزمون |
---|
Shore hardness | Shore A | ASTM D2240 | 76 |
Supplementary Information | شرایط آزمون | روش آزمون | نتیجه آزمون |
---|
MDR | 最小转矩 | ASTM D6601 | 0.16 N·m |
MS | MV | ASTM D1646 | 28 MU |
MS | t15 | ASTM D1646 | 24.0 min |
sulfurization | t'90 | ASTM D2084 | 3.5 min |
sulfurization | ts2 | ASTM D2084 | 2.0 min |
sulfurization | 最大转矩 | ASTM D2084 | 15 N·m |
sulfurization | 最小转矩 | ASTM D2084 | 1.5 N·m |
Test compound | Ca(OH)2 | | 6 % |
Test compound | MgO–DE | | 3 % |
Test compound | N-990MT炭黑 | | 30 % |
Test compound | Tecnoflon®FORTF636 | | 100 % |
MDR | t'50 | ASTM D6601 | 1.4 min |
MDR | t'90 | ASTM D6601 | 2.1 min |
MDR | ts2 | ASTM D6601 | 1.2 min |
MDR | 最大转矩 | ASTM D6601 | 3.0 N·m |
elastomer | شرایط آزمون | روش آزمون | نتیجه آزمون |
---|
tensile strength | 100%应变 | ASTM D412 | 8.20 MPa |
tensile strength | | ASTM D412 | 18.4 MPa |
elongation | Break | ASTM D412 | 170 % |
Thermal performance | شرایط آزمون | روش آزمون | نتیجه آزمون |
---|
Temperature recovery characteristics | TR10 | ASTM D1329 | -19 °C |
Temperature recovery characteristics | TR30 | ASTM D1329 | -14 °C |
Temperature recovery characteristics | TR50 | ASTM D1329 | -10 °C |