برگه داده فنی
physical property | شرایط آزمون | روش آزمون | نتیجه آزمون |
---|---|---|---|
density | ASTM D792 | 0.918 g/cm³ | |
melt mass-flow rate | 190°C/2.16kg | ASTM D1238 | 1.0 g/10min |
optical performance | شرایط آزمون | روش آزمون | نتیجه آزمون |
---|---|---|---|
gloss | 45°,50.8µm | ASTM D2457 | 54 |
Haze ratio | 50.8µm | ASTM D1003 | 15 % |
Mechanical properties | شرایط آزمون | روش آزمون | نتیجه آزمون |
---|---|---|---|
coefficient of friction | Itself - Dynamic | ASTM D1894 | 0.091 |
Itself - Static | ASTM D1894 | 0.11 |
film | شرایط آزمون | روش آزمون | نتیجه آزمون |
---|---|---|---|
film thickness | 50 µm | ||
Thin film puncture strength | 50µm | 内部方法 | 6.62 J/cm³ |
Secant modulus | 2%正割,MD:50µm | ASTM D882 | 165 MPa |
2%正割,TD:50µm | ASTM D882 | 170 MPa | |
tensile strength | MD:屈服,50µm | ASTM D882 | 8.70 MPa |
TD:屈服,50µm | ASTM D882 | 9.40 MPa | |
MD:断裂,50µm | ASTM D882 | 30.3 MPa | |
TD:断裂,50µm | ASTM D882 | 28.8 MPa | |
elongation | MD:断裂,50µm | ASTM D882 | 700 % |
TD:断裂,50µm | ASTM D882 | 750 % | |
Dart impact | 50µm | ASTM D1709A | 640 g |
Elmendorf tear strength | MD:50µm | ASTM D1922 | 920 g |
TD:50µm | ASTM D1922 | 1200 g |