ABS Toyolac® 700-X01 TORAY MALAYSIA
59
- ویژگیها:درخشش بالا
- کاربردها:لوازم الکتریکیاسباب بازیکاغذ نوشتاری
- گواهینامهها:UL
برگه داده فنی
| impact performance | شرایط آزمون | روش آزمون | نتیجه آزمون |
|---|---|---|---|
| Impact strength of cantilever beam gap | 23°C,12.7mm | ASTM D256 | 200 J/m |
| 23°C,3.20mm | ASTM D256 | 220 J/m | |
| 0°C,12.7mm | ASTM D256 | 110 J/m | |
| 0°C,3.20mm | ASTM D256 | 160 J/m | |
| -30°C,12.7mm | ASTM D256 | 80 J/m | |
| -30°C,3.20mm | ASTM D256 | 110 J/m | |
| Charpy Notched Impact Strength | 23°C | ISO 179/1eA | 18 kJ/m² |
| flammability | شرایط آزمون | روش آزمون | نتیجه آزمون |
|---|---|---|---|
| UL flame retardant rating | UL 94 | HB |
| mechanical properties | شرایط آزمون | روش آزمون | نتیجه آزمون |
|---|---|---|---|
| bending strength | ISO 178 | 77.0 Mpa | |
| ASTM D790 | 73.0 Mpa | ||
| Bending modulus | ASTM D790 | 2300 Mpa | |
| Tensile modulus | ISO 527-2/1 | 2600 Mpa | |
| tensile strength | Yield | ASTM D638 | 46.0 Mpa |
| Yield | ISO 527-2/50 | 51.0 Mpa | |
| elongation | Break | ASTM D638 | 15 % |
| Tensile strain | Break | ISO 527-2/50 | >10 % |
| thermal performance | شرایط آزمون | روش آزمون | نتیجه آزمون |
|---|---|---|---|
| thermal conductivity | ASTMC177 | 0.16 W/m/K | |
| Linear coefficient of thermal expansion | MD | ASTM D696 | 7.2E-05 cm/cm/°C |
| Hot deformation temperature | 1.8MPa,Unannealed | ISO 75-2/A | 81.0 °C |
| 1.8MPa,Unannealed,12.7mm | ASTM D648 | 92.0 °C | |
| 1.8MPa,Unannealed,6.40mm | ASTM D648 | 86.0 °C |
| Physical properties | شرایط آزمون | روش آزمون | نتیجه آزمون |
|---|---|---|---|
| Water absorption rate | 23°C,24hr | ASTM D570 | 0.30 % |
| Shrinkage rate | MD | ASTM D955 | 0.40-0.60 % |
| melt mass-flow rate | 220°C/10.0kg | ISO 1133 | 40 g/10min |
| density | ISO 1183 | 1.04 g/cm³ | |
| ASTM D792 | 1.05 g/cm³ |
| Electrical performance | شرایط آزمون | روش آزمون | نتیجه آزمون |
|---|---|---|---|
| Dissipation factor | 1kHz | ASTM D150 | 6.2E-03 |
| Dielectric constant | 1kHz | ASTM D150 | 3.10 |
| Dielectric strength | ASTM D149 | 23 KV/mm | |
| Volume resistivity | 23°C | ASTM D257 | >1.0E+16 ohms·cm |
| Surface resistivity | ASTM D257 | >1.0E+16 ohms |
| hardness | شرایط آزمون | روش آزمون | نتیجه آزمون |
|---|---|---|---|
| Rockwell hardness | R-Scale | ASTM D785 | 114 |
نکات مهم: Plas.com دادههای برگه فنی را از تولیدکنندگان مواد جمعآوری کرده است. Plas.com تمام تلاش خود را برای افزایش دقت دادهها انجام میدهد، اما هیچ مسئولیتی در قبال دادهها ندارد. اکیداً توصیه میشود که صحت دادهها را با تولیدکنندگان مواد تأیید کنید پیش از آنکه تصمیم نهایی بگیرید.