| optical performance | شرایط آزمون | روش آزمون | نتیجه آزمون | واحد آزمایش |
|---|---|---|---|---|
| transmissivity | 250μm | ASTM D1003 | 93.0 | % |
| turbidity | 250μm | ASTM D1003 | 0.80 | % |
| Huangdu Index | 250mm | ASTM D1925 | 0.50 | YI |
| UV Transmittance | 250.0μm | 89 | % | |
| gloss | 60°,250μm | ASTM D2457 | 158 | |
| Refractive index | ASTM D542 | 1.540 | ||
| elastomer | شرایط آزمون | روش آزمون | نتیجه آزمون | واحد آزمایش |
| tear strength | Split6 | ASTM D1938 | 9.0 | kN/m |
| Split7 | ASTM D1938 | 10 | kN/m | |
| mechanical properties | شرایط آزمون | روش آزمون | نتیجه آزمون | واحد آزمایش |
| Taber wear resistance | 23°C,250.0μm | ASTM D1044 | 20Haze | % |
| thermal performance | شرایط آزمون | روش آزمون | نتیجه آزمون | واحد آزمایش |
| Melting temperature | 119 | °C | ||
| Linear coefficient of thermal expansion | MD:23°C | ASTM D696 | 8E-05 | cm/cm/°C |
| specific heat | 60°C | DSC | 1700 | J/kg/°C |
| 100°C | DSC | 1900 | J/kg/°C | |
| 150°C | DSC | 2300 | J/kg/°C | |
| 200°C | DSC | 2400 | J/kg/°C | |
| 250°C | DSC | 2600 | J/kg/°C | |
| Physical properties | شرایط آزمون | روش آزمون | نتیجه آزمون | واحد آزمایش |
| density | ASTM D792 | 1.19 | g/cm³ | |
| Water absorption rate | 23°C,24hr,0.254mm | ASTM D570 | 0.50 | % |
| film | شرایط آزمون | روش آزمون | نتیجه آزمون | واحد آزمایش |
| tear strength | MD:23°C,250.0μm | ASTM D1938 | 310 | gf |
| TD:23°C,250.0μm | ASTM D1938 | 200 | gf | |
| Dart impact | -30°C,250μm | ASTM D1709A | 830 | g |
| -18°C,250μm | ASTM D1709A | 830 | g | |
| 23°C,250μm | ASTM D1709A | 830 | g | |
| Tear resistance of pants type | MD:250μm | ISO 6383-1 | 10.0 | N/mm |
| TD:250μm | ISO 6383-1 | 9.00 | N/mm | |
| Oxygen permeability | 23°C,250μm,50%RH | ASTM D3985 | 44 | cm³·mm/m²/atm/24hr |
| Water vapor permeability | 23°C,100%RH,250μm | ASTMF1249 | 4.0 | g/m²/24hr |
| 38°C,100%RH,250μm | ASTMF1249 | 10 | g/m²/24hr | |
| Carbon dioxide transmittance | 23°C,254.0μm | ASTM D1434 | 210 | cm³·mm/m²/atm/24hr |
| Elmendorf tear strength | MD:23°C,250.0μm | ASTM D1922 | 4 | N |
| tensile strength | Yield,250μm | ASTM D882 | 41.0 | MPa |
| Break,250μm | ASTM D882 | 57.0 | MPa | |
| Break,250μm | ASTM D882 | 42.0 | MPa | |
| Tensile strain | Yield,250μm,MD | ASTM D882 | 8.0 | % |
| Yield,250μm | ASTM D882 | 8.0 | % | |
| elongation | Break,250μm | ASTM D882 | 110 | % |
| Tensile strain | Break,250μm | ASTM D882 | 120 | % |
| Elmendorf tear strength | TD:23°C,250.0μm | ASTM D1922 | 4 | N |
| PPTTearResistance | MD:23°C,250.0μm | ASTM D2582 | 40 | N |
| TD:23°C,250.0μm | ASTM D2582 | 40 | N | |
| film thickness | 250 | µm | ||
| Thin film puncture strength | 250μm | ASTM D3763 | 4.50 | J |
| Secant modulus | 250μm,MD | ASTM D882 | 1500 | MPa |
| 250μm,TD | ASTM D882 | 1400 | MPa | |
| tensile strength | Yield,250μm | ASTM D882 | 43.0 | MPa |
| Supplementary Information | شرایط آزمون | روش آزمون | نتیجه آزمون | واحد آزمایش |
| SurfaceEnergy | Dispersive:23°C,250.0μm | ASTM D5946 | 39 | dyne/cm |
| Polar:23°C,250.0μm | ASTM D5946 | 8 | dyne/cm | |
| Total:23°C,250.0μm | ASTM D5946 | 47 | dyne/cm |