| thermal performance | شرایط آزمون | روش آزمون | SABIC INNOVATIVE CHONGQING/MC1300-100 |
|---|---|---|---|
| Hot deformation temperature | 0.45 MPa, Unannealed, 3.20 mm | ASTM D648 | 115 °C |
| 1.8 MPa, Unannealed, 3.20 mm | ASTM D648 | 98.0 °C | |
| Linear coefficient of thermal expansion | Across Flow : -40 to 40°C | ASTM E831 | 9.0E-5 cm/cm/°C |
| Flow : -40 to 40°C | ASTM E831 | 7.2E-5 cm/cm/°C | |
| thermal conductivity | ASTM C177 | 0.20 W/m/K | |
| Vicat softening temperature | ASTM D15255 | 111 °C |
| mechanical properties | شرایط آزمون | روش آزمون | SABIC INNOVATIVE CHONGQING/MC1300-100 |
|---|---|---|---|
| Bending modulus | 50.0 mm Span | ASTM D790 | 2060 Mpa |
| bending strength | Yield, 50.0 mm Span | ASTM D790 | 72.0 Mpa |
| elongation | Yield | ASTM D638 | 8.6 % |
| Break | ASTM D638 | 150 % | |
| Tensile modulus | ASTM D638 | 2130 Mpa | |
| tensile strength | Yield | ASTM D638 | 50.0 Mpa |
| Break | ASTM D638 | 44.0 Mpa |
| Physical properties | شرایط آزمون | روش آزمون | SABIC INNOVATIVE CHONGQING/MC1300-100 |
|---|---|---|---|
| melt mass-flow rate | 260°C/5.0 kg | ASTM D1238 | 14 g/10 min |
| Shrinkage rate | Across FlowFlow : 3.20 mm | Internal Method | 0.50 - 0.70 % |
| Flow : 3.20 mm | Internal Method | 0.50 - 0.80 % | |
| Water absorption rate | 24 hr | ASTM D570 | 0.10 % |
| impact performance | شرایط آزمون | روش آزمون | SABIC INNOVATIVE CHONGQING/MC1300-100 |
|---|---|---|---|
| Dart impact | -30°C, Total Energy | ASTM D3763 | 33.0 J |
| 23°C, Total Energy | ASTM D3763 | 40.0 J |
| injection | شرایط آزمون | روش آزمون | SABIC INNOVATIVE CHONGQING/MC1300-100 |
|---|---|---|---|
| Back pressure | 0.300 to 0.700 Mpa | ||
| drying temperature | 100 to 105 °C | ||
| drying time | 3.0 to 4.0 hr | ||
| Exhaust hole depth | 0.038 to 0.076 mm | ||
| Mold temperature | 75 to 100 °C | ||
| Processing (melt) temperature | 260 to 290 °C | ||
| Screw speed | 40 to 70 rpm | ||
| Spray nozzle temperature | 260 to 290 °C | ||
| Suggested injection volume | 30 to 80 % | ||
| Suggested maximum moisture content | 0.020 % | ||
| Temperature at the front of the material cylinder | 255 to 290 °C | ||
| Temperature at the rear of the barrel | 250 to 280 °C | ||
| Temperature in the middle of the barrel | 255 to 290 °C |